二氧化硅包裹锐钛矿型二氧化钛处理木材的老化性能研究
2025-08-03尤梓媛于洋贺增成肖泽芳张天鹏谢延军邱哲
关键词:速生杨木;抗老化;二氧化钛;表面修饰;木材改性;紫外屏蔽;光降解;自由基中图分类号:S781.7 文献标识码:A DOI: 10.7525/j.issn.1006-8023.2025.04.006
Abstract:To enhance the weathering resistance of wood,anatase titanium dioxide was encapsulated with silica to form silica-coated anatase-type titanium dioxide (A-TiO 2 @Si0 2 ),which was then modified with a silane coupling agent to produce the modifier(KH560-TiO2@SiO 2 ).KH560 referred to γ -glycidoxypropyltrimethoxysilane.Fast-growing poplar wood was treated with this modifier via vacuum impregnation,and the effects of KH560-TiO 2 @SiO
on the ultraviolet resistance ofpoplarwood were systematicalyevaluated.Theresults indicated thatTiandSi elements were introduced into the surface of the modified wood,with asignificant amount of particulate materbeing loaded.The treated wood exhibitedahighercontactanglecomparedtotheuntreated wood,whichhelpedtoreduce thedegradationcaused bywater in outdoor applications.Theabilityofthe modifiedwood to excitehydroxylradicals,superoxideanions,and phenoxylradicals was reduced,while its absorbance in the UV region increased.Untreated poplar wood experienced rapid lignin degradationafter UVaging,leading to photodegradationand structural deterioration.The photocatalytic propertiesof anatase titanium dioxide (A-TiO 2 )promoted the degradation of cellulose in poplar wood. However,the KH560-TiO 2 @Si0 2 modificationdelayed lignindegradation whilemaintainingthestabilityofcellose.Insummary,theencapsulation treatment reduced the photocatalytic activity of A-TiO 2 ,and the modifier acted as a UV shield while decreasing the wettability of the wood,thereby enhancing the weathering resistance ofpoplar wood.Fast-growing poplar wood treated with KH560- TiO2@Si0 2 has the potential for outdoor applications.
KeyWords:Fast-growing poplar;weathering;titanium dioxide;surface modification;wood modification;ultraviolet shielding;photodegradation; free radical
0 引言
二氧化钛 (TiO2) 凭借其独特的物理化学特性,在增强木材耐老化性能方面具有优异的效果,逐渐成为一种常见的木材涂料组分及木材改性剂[1-2]。然而,TiO2 并非以单一的形态存在,其具有锐钛矿型、金红石型等在内的多种晶型结构,不同晶型在性能上存在着显著差异,进而会对木材产生不同的老化防护效果[3-4]。锐钛矿型二氧化钛 (A-Ti02 是一种优良的紫外吸收剂,能够吸收波长较短的紫外光,特别是长波紫外线(UVA)和中波紫外线(UVB)波段的光线[5-6]。但同时,其高光催化活性可能会对木材抗老化改性造成负面影响[7-8]。在光照条件下, A-TiO2 能够产生具有强氧化性的自由基,这些自由基反而会加速木材的降解过程[9]。因此,如何在保留 A-TiO2 抗紫外性能的同时,有效抑制其光催化性能,成为 A-TiO2 在木材抗老化改性领域应用中亟需解决的问题。
工业上广泛采用二氧化硅(
作为 TiO2 光催化活性的抑制剂。具体而言,通过控制二氧化硅前驱体在碱性环境下的水解过程,可以在 TiO2 与二氧化硅前驱体表面之间构建出Ti一O一Si化学键。随后,通过SiO2 之间的表面羟基在不断靠近的过程中发生脱水缩合生成Si一O一Si键,构建出三维网络结构,从而在TiO2 表面形成均匀致密覆盖的 SiO2 壳层,减少 TiO2 与水和氧气的接触,进而抑制其光催化性能[10-11]
本研究以正硅酸乙酯(TEOS)为前驱液,在 A-TiO2 纳米颗粒表面构建致密的 SiO2 壳层 (A-TiO2@SiO2 )为进一步提高改性木材的疏水性,利用 γ -缩水甘油基氧基丙基三甲氧基硅烷(KH560)对 A-TiO2@SiO2 进行表面处理,最后对杨木进行浸渍改性。……