APP下载

Microstructure and heat treatment for Ni3Al-based single crystal alloy with different crystal orientations

2020-07-29LiwuJingXuezhengDouMeilingWuMinCi

Liwu Jing ,Xuezheng Dou ,Meiling Wu ,Min Ci

a National Center for Materials Service Safety,University of Science and Technology Beijing,Beijing,100083,China

b NCS Testing Technology Co.,Ltd.,Beijing,100081,China

c Beijing Institute of Aeronautical Materials,Beijing,100095,China

d Avic Manufacturing Technology Institute,Beijing,100024,China

Keywords:Ni3Al-Based Single crystal superalloy Crystal orientation Heat treatment IC6SX

ABSTRACT Ni3Al-based single crystal alloy IC6SX with different crystal orientations were prepared by seed crystal method.The microstructure and heat treatment of the alloy were investigated.The results showed that the microstructure of the alloy was in dendrite structure,and the crystal orientation had significant effect on the dendrite morphology of this alloy.The precipitated phases of(MoNi)6C and NiMo appeared in the microstructure of the three alloys with different crystal orientations during solidification process.Compared with other two alloys,the volume fractions of precipitated phases of both (MoNi)6C and NiMo was the most in the alloy with [111]orientation and the least in the alloy with [001]orientation.The solidus and liquidus temperatures of the alloy IC6SX tested by differential scanning calorimetry(DSC)were 1356°C and 1387°C,respectively.Meanwhile,the effect of different solution temperatures on the microstructure of the alloy with different orientations was studied.The results showed that the precipitated phases of (MoNi)6C and NiMo were eliminated with the solid solution treatment under the condition of 1300°C/10 h.However,the incipient melting of the alloys occurred due to the dissolution of low melting point phases.As the temperature dropped to 1280°C,the area of incipient melting in the alloy with different orientations decreased gradually.However,there was no incipient melting appearing in the three alloys with different orientations when the solution treatment temperature dropped to 1260°C.∗Corresponding author.

1.Introduction

With the development of aviation industry,the structure and properties of aero-engines are improved constantly.Accordingly,the working temperature and requirements for the properties of superalloy turbine blades also increased continuously [1].Ni3Al-based single crystal superalloy has the advantages of low density,high melting point,large specific strength,high plasticity,good mechanical properties at high temperature and strong oxidation resistance.And therefore the research and development on Ni3Al-based single crystal superalloys has been become a research hotspot in the field of high-temperature structural materials [2–4].

The researches in China on Ni3Al-based materials have achieved certain results during the last decades,and several Ni3Al-based superalloys with excellent properties have been developed for turbine blades and vanes of aero-engines,such as IC6,IC6A,IC10 and IC6SX[5].And the single crystal Ni3Al-based superalloy IC6SX has been developed on the basis of DS IC6 which is the directionally solidified alloy with similar contents for further increasing mechanical properties [6].IC6SX has low density,high initial melting point,high temperature durable strength,low cost,and good comprehensive properties [7].Previous research results [8,9] showed that nickel-based single crystal alloys grow along with different orientations have the different dendrite morphology.The dendrites of the alloy with[001]orientation have the shape of a cross,distributed uniformly and irregularly on the cross sections.And the dendrites of the alloy with [011] orientation are regularly arranged in rows on the cross sections.However,there is a certain angle between the dendrite arms for the alloy with [111] orientation,and the dendrites show a scissor-like distribution.The result of Li et al.[10] showed that after high temperature heat treatment of 1280 °C/10 h,air cooling+870 °C/32 h the dendrite structure of IC6SX disappeared,and the creep rupture life significantly increased.It has been found that the effect of solid solution heat treatment on the microstructure,size and shape of grains for the nickel-based single crystal alloys are significant [11].However,the effect of the heat treatment on the microstructure and mechanical properties of Ni3Albased single crystal alloy IC6SX with different crystal orientations has not been carried out.

In this paper,Ni3Al-based single crystal alloy IC6SX specimens with different crystal orientations were prepared by seed crystal method[12].And the effect of crystal orientations and solid solution temperature on the microstructure of the alloy was explored,providing a theoretical basis for the application of Ni3Al-based single crystal alloy.

2.Experimental procedure

The material used for the present study was a Ni3Al based alloy IC6SX,with a nominal composition of Ni-7.4–8.0Al-13.5–14.3Mo-0.02–0.03B(wt%).The raw materials used were all high-purity elements,including Ni (99.9%),Al (99.9%) and Mo (99.9%).Firstly,the master alloy ingot with size of φ75×500 mm was prepared by vacuum induction melting method in the GVR-100 vacuum induction furnace.Then the single crystal alloy test bars with different crystal orientations were prepared by seed crystal method in the DZG-0.025 directional solidification furnace,and the size of the test bars were φ15×160 mm.All the test bars were calibrated for crystal orientation by X-ray backscattering Laue method.The test bars with orientation deviation less than 5° and without defects were selected for this study.

The microstructure of the specimens was analyzed by optical microscope (OM) and scanning electron microscope (SEM).The differential thermal analysis was performed for the specimens by TGA/STDA851 differential thermal analyzer.The sample size was φ5×0.5 mm and the heating rate was 10°C/min.The heat treatment was carried out by KSY-8-16A high temperature resistance furnace.The phase composition was determined by Rigaku 2500 X-ray diffractometer.The precipitated phases in the alloy were obtained by extraction method.The extract liquor was composed of methanol,hydrochloric acid and tartaric acid.The volume fraction of precipitated phases in alloy was calculated by“grid method”.At least,5 photos from different areas of the specimens were selected for statistic analysis.The formula for calculating the volume fraction is:PP=P/PT.In the formula,PTis the total number of grid intersection points;P is the number of measured objects falling on the grid intersection.

3.Results and discussion

3.1.Effects of crystal orientation on as-cast microstructure

Fig.1 shows the three-dimensional reconstruction for the as-cast microstructure of IC6SX alloy with different crystal orientations.It can be found that the three-dimensional structure and morphology were characterized clearly.And it can be seen that the single crystal alloys with different orientations were all dendrite structure,but the crystal orientation had a significant impact on the dendrite morphology of the alloy.For the single crystal alloy with [001] orientation,there was a typical dendrite morphology parallel to the [001] orientation,a "+"shaped dendrite morphology in regular arrangement appeared on(001)plane,and primary dendrite arranged on both (010) and (100) planes.It may be due to the preferred growth direction of [001] crystal orientation of the single crystal alloy parallel to the heat flow direction.The primary dendrites grew in the opposite direction of heat flow.With the primary dendrites growing continuously,the secondary dendrites grew symmetrically like the arms of the primary dendrites.The secondary dendrites were perpendicular to each other and the morphology of "+" shaped dendrite with regular arrangements formed.

For the dendrite morphology of the alloy with[011]orientation,the preferred growth direction[001]crystal orientation was not parallel to the direction of heat flow,and there was a 45°angle between them.At this time,the dendrites would grow by turns in two mutually preferred directions and the angle between secondary dendrites was about 60°.For the single crystal alloy with [111] orientation,the dendrites also showed staggered growth.It was measured that the eutectic phase volume fraction of the three alloys with [001],[011] and [111] orientation were about 4.5%,4.8%and 6.38%,respectively.It was known that [NiMo]6C and NiMo precipitated phases were distributed at interdendritic region.And the dendritic spatial configuration of the alloy with [111] orientation was the most complicated,which would cause the highest proportion of dendrite gaps.Therefore,for the alloy with[111] orientation,the eutectic phase volume fraction was maximum.However,the dendrites were just along one direction in the alloy with[001] orientation where the proportion of dendrite gaps was least,therefore the content of precipitated phases might be minimum.

3.2.Interdendritic eutectic structure

There were a large number of interdendritic eutectic structures in the three alloys with different orientations.The EDS results showed that the basic composition of the eutectics for the single crystal alloys with three different orientations were the similar.In addition,the morphology of the three alloys were also similar.The typical morphology of interdendritic eutectic structure of the alloy IC6SX with [001] orientation is displayed in Fig.2.

Fig.2(a) showed that the black eutectic structure distributed at interdendritic zones,and there were some white elliptical-shape phases in the eutectic structure.The black-and-white lamellar structure and the black elliptical-shape phase in the eutectic structure were observed by SEM,as shown in Fig.2(b)and(c).Meanwhile,it was also found that the eutectic structure was surrounded by the fine white phases from Fig.2(c).From the EDS results,it was confirmed that both the fine white phases and the black elliptical-shaped phase were γ′ phase,and that the white lamellar eutectic region was rich in Mo and Ni elements,as shown in Fig.2(d).

Fig.1.Three-dimensional reconstruction graph for the as-cast microstructure of IC6SX alloy with different crystal orientations (a) [001] orientation;(b)[011]orientation;(c)[111] orientation.

Fig.2.Eutectic structure of IC6SX alloy with [001] orientation.(a) Low multiple eutectic structure (OM);(b) Low multiple eutectic structure (SEM);(c) partial enlarged detail from (b)(SEM);(d) EDS energy spectrum curve for the white phase from (c).

In order to identify the composition of the phases in the eutectic,the phases extraction of as-cast single crystal alloy IC6SX was carried out.Fig.3 shows the three-dimensional morphology of the extraction phase under scanning electron microscopy.In Fig.3(a),the phases in the eutectic region were mainly composed of block phases with a certain geometry.Fig.3(b) shows that the bulk phase consisted of white contrast phase and gray contrast phase.According to the EDS results,the bulk phase was mainly enriched with Mo and Ni elements in the ratio closed to 1:1.In order to further determine the type of phases in the eutectic,the extracted powder was collected for XRD identification.The XRD result is shown in Fig.3(c).It was identified that the phase composition in the eutectic region was mainly NiMo phase and (MoNi)6C phase.

Fig.3.Three-dimensional morphology of extraction phase remaining on the matrix after extraction.(a)Extraction phase between dendrites (SEM image);(b)Extraction phase between dendrites (BSE image);(c) XRD pattern of the powder after extraction.

Fig.4.DSC curve for the heating process of Alloy IC6SX.

3.3.Heat treatment for single crystal alloy IC6SX

3.3.1.DSC analysis

Fig.4 shows the DSC heating curve of as-cast single crystal alloy IC6SX.From Fig.4,the solidus temperature and liquidus temperatures were identified to 1356°C and 1387°C,respectively.It should be noted especially that there is a peak appearing in temperature ranges from 1250°C to 1270°C before reaching the main endothermic peak temperature.It indicated that an endothermic transition occurred in this temperature range.And this temperature range could be the solid solution temperature of γ′ phase.

3.3.2.Microstructure analysis for IC6SX after solid solution heat treatment

Since the microstructure is mainly related to heat treatment process and not affected by the crystal orientation,the single crystal alloys IC6SX with [001] orientation was as an example to investigated.In order to eliminate eutectic structure and reduce dendrite segregation,the solid solution heat treatment is necessary.In addition,the incipient melting has to be avoided during solid solution heat treatment.Generally,the solid solution heat treatment temperature selected for single crystal alloy was lower than its solidus temperature by 50°C.According to the phase transition temperature as mentioned above in Fig.4,the solid solution heat treatment process for the three alloys were carried out at 1300°C/10 h,1280°C/10 h and 1260°C/10 h,respectively.

Fig.5(a) showed the microstructures of the IC6SX alloy with [001]orientation after the solid solution treatment under the condition of 1300°C/10 h.It can be seen from Fig.5(a) that the eutectics were eliminated basically,alone with a few portion of initial melting.

Fig.5(b) displayed the microstructure of single crystal alloy IC6SX with [001] orientation after the solid solution treatment under the condition of 1280°C/10 h.From Fig.5(b),the initial melting area reduced compared with that shown in Fig.5(a).Fig.5(d)and(f)show the initial melting microstructure after the solid solution treatment under the condition of 1280°C/10 h.From Fig.5(d),it was found that the initial melting area was gray-white elliptical structure.The formation of the abnormal structure probably resulted from that the low melting point phase underwent the initial melting to form the part of liquid metal which was re-solidified during the cooling process.Further observation showed that the structure of the elliptical initial melting area was consisted of the white and gray phase surrounded by coarse γ′phase and the fine two-phase structure of γ’ and γ,as shown in Fig.5(e)~(f).

Fig.5(c)shows the microstructure of single crystal alloy IC6SX with[001]orientation after the solid solution treatment under the condition of 1260°C/10 h.From Fig.5(c),it can be indentified that there was no primary melting to occur,however the eutectic phases between the dendrites were not eliminated completely.From the SEM images in Fig.6(a),it can be found that the single crystal alloy was not completely solid-dissolved,and there were still large γ′ phase existing at the dendrite arm area because of the incomplete solid solution.The size of the large γ′ phase was about 2.2 μm at the dendrite arm.Fig.6(b) shows that the γ′phase in the interdendrite region became homogeneous,and the γ′ phase size was about 1.3 μm at interdendrite region.Compared with the microstructure of as-cast alloy,both the initially coarse γ′phase and the fine γ′ phase in the interdendrites region disappeared after heat treated at 1260°C/10 h.However,the large white and gray phases were still found as shown in Fig.6(c).The reason may be that during the solid solution treatment the smaller phase dissolved and disappeared,while the larger white NiMo phase and the gray(MoNi)6C phase were not completely solid-dissolved into the matrix.

Based on the above results that to ensure the elimination of the eutectic structure without initial melting,the solid solution heat treatment process parameter for the single crystal alloy IC6SX is decided to 1260°C/10 h.

3.3.3.Aging heat treatment of the alloy IC6SX

Generally,after solid solution heat treatment,the composition and microstructure of the single crystal alloy become more homogeneous,which will improve the strength significantly with the obvious decrease of the ductility.In order to obtain excellent comprehensive properties,the aging heat treatment for the single crystal superalloy is necessary after solid solution treatment.Based on the aging heat treatment process for directionally solidified Ni3Al-based alloy IC6,the aging heat treatment of single crystal alloy IC6SX was selected under 870°C/32 h.The typical microstructure of single crystal alloy IC6SX with three different orientations after solid solution and aging heat treatment are shown in Fig.7.Compared with the microstructures after solid solution treatment,the γ′ phase became more cubic.The size and the volume fraction of γ′ at the dendrite arm with incomplete solid solution was about 2.1 μm and 81.4%,respectively.The size and the volume fraction of γ′at interdendrite region was about 0.85 μm and 76.7%,respectively.Meanwhile,a small amount of white phase was found,which should be the fine Y–NiMo phase as reported earlier [13].Since the aging heat treatment temperature was within the transition temperature range of Y–NiMo phase,the reaction equation for the γ phase was γ→Y–NiMo+γ′.After the aging heat treatment,the size and shape of the primary bulk white and gray phase at interdendrite region did not change,and its percentage in the three alloys with [001],[011] and [111] orientations were 1.3%,1.1% and 1.7%,respectively.

The dissolved phase at interdendrite region after solid solution treatment and aging heat treatment was confirmed by XRD.The XRD pattern was shown in Fig.8.In contrast to the as-cast alloy IC6SX,the type of the residual phases at interdendrite region did not change after the solid solution and aging heat treatment,which were still the block white NiMo phases and the gray (MoNi)6C.

3.4.Analysis and discussion

During the preparation of single crystal alloy,the temperature at the phase interface increases with the release of latent heat of crystallization under the condition of negative temperature gradient,which leads that the liquid phase is in the supercooling condition.The liquidsolid interface will form many branches extending toward the liquid,and all these branches will grow along with a certain crystallographic axis.Meanwhile,the secondary dendrites may branch out from these dendrites,and tertiary dendrites may branch out from the secondary dendrites.The primary dendrites in the vertical section with [001]orientation grow in parallel along the axis,while the secondary dendrites are perpendicular to the primary dendrites.The vertical and cross sections with[011]and[111]orientations are all double cross dendrite morphology,where the morphology and arrangement of dendrites are obviously different from that with [001] orientation.Since the single crystal alloy with three orientations and all crystallize in the growth mode of dendrites during the cooling process,non-equilibrium solidification will result in the components different between the first crystallized dendrite trunk and the later crystallized dendrites.The element Al is a negative segregation element and mainly enriched in the dendrite area.While Mo is a positive segregation element,it mainly enriched at interdendrite region.Compared with the γ′ phase between core and inter dendrites,the number of γ′ phase at dendrite area is larger and the morphology is coarser.

Fig.5.Microstructure of IC6SX alloy with[001]orientation after solid solution treatment(OM image).(a)1300°C/10 h;(b)1280°C/10 h;(c)1260°C/10 h;Initial melting microstructure of IC6SX alloy after solid solution treatment (1280°C/10 h).(d)Initial melting area (OM photo);(e) Low multiple initial melting area (SEM image);(f) High multiple initial melting area (BSE image).

Eutectic structure forms in the process of non-equilibrium crystallization.When the solidification temperature of the alloy is maintained at a temperature slightly lower than the eutectic point,it will lead the composition in the eutectic region to be close to the alloy nominal composition by diffusion.In the condition of higher temperature for a long time,the alloying elements diffuse uniformly,and the dendrite segregation is eliminated basically.In contrast to the solid solution treated microstructures of the alloys with different orientations,it can be found that the microstructure transformation has weak relation with the crystal orientation of the alloy,however it mainly depends on the composition of the alloy itself.The microstructure study of as-cast and heat-treated alloys showed that in as-cast alloy there were larger γ′phase at the dendrite area,fine γ′ phase at interdendrite area and primary coarse γ′phase in eutectic area.It has been found that the γ′phase formed during the aging treatment.Except for a small amount of larger γ′ phase at the dendrite area,which is not completely solid-dissolved,the γ′phases in other areas were uniform in size.In addition,after solid solution treatment,the smaller size of the hard and brittle phases in the eutectic structure region in the as-cast dendrites disappeared gradually due to the element diffusion.Meanwhile,the larger size hard and brittle phases were not eliminated completely.

4.Conclusions

1) Single crystal alloys with different orientations have different growth mode and dendrite morphologies.The primary dendrites of single crystal alloy with [001] orientation grow along the axial direction.However the dendrite morphology of single crystal alloys with [011] and [111] orientations are more complicated,and there is a certain angle between the direction of dendrite growth and heat flow.There are lamellar (MoNi)6C and NiMo phases in the dendrite area of all three alloys.

2) Solid solution treatment can effectively eliminate the element segregation and the eutectic phase.The initial melting of single crystal alloy IC6SX occurs at 1280 °C or above.After the heat treatment under the condition of 1260 °C/10 h+870 °C/32 h,the γ′ phase becomes uniform and regular except for a small amount of incompletely solved γ′phase at the dendrite arm.The primary coarser phases of(MoNi)6C and NiMo in the dendrites cannot be completely eliminated by heat treatment.

3) After heat treatment,the microstructure of the single crystal alloy IC6SX with different crystal orientations is basically the same.And the heat treatment system is independent on the crystal orientation.

Fig.6.Microstructure of IC6SX alloy with [001] orientation after solid solution treatment (1260°C/10 h).(a) Dendrite stem structure;(b) Interdendrite structure(SEM image);(c) White phase and gray phase between dendrites (BSE image).

Fig.7.SEM images showing the microstructure of single crystal alloy after solid solution and aging treatment under 1260°C/10 h (a1) Dendrite stem;(a2)Interdendrite;(a3) Eutectic with [001] orientation;(b1) Dendrite stem;(b2)Interdendrite;(b3) Eutectic with [011] orientation;(c1) Dendrite stem;(c2)Interdendrite;(c3) Eutectic with [111] orientation.

Fig.8.XRD results after solid solution,aging treatment and phase extraction.

Declaration of competing interest

The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper.

Acknowledgments

This research was financial supported by the National Science and Technology Major Project (Grant NO.2017-VI-0012-0084,2017-VI-0011-0083),the Fundamental Research Funds for the Central Universities (Grant NO.FRF-GF-19-029B) and the National Natural Science Foundation of China (Grant NO.51471022).


登录APP查看全文