Dynamic recrystallization and phase transformation behavior of a wrought β-γ TiAl alloy during hot compression

2020-07-29LeiZhuJinshnLiBinTngFengtongZhoKeHuShopengYnHongchoKou

Lei Zhu ,Jinshn Li ,Bin Tng,b,∗ ,Fengtong Zho ,Ke Hu ,Shopeng Yn ,Hongcho Kou

a State Key Laboratory of Solidification Processing,Northwestern Polytechnical University,127 Youyixi Road,Xi'an,710072,China

b Shaanxi Key Laboratory of High-Performance Precision Forming Technology and Equipment,Northwestern Polytechnical University,Xi'an,Shaanxi,710072,China

Keywords:β-γ TiAl alloy Hot compression Dynamic recrystallization Microstructure Phase transformation

ABSTRACT The dynamic recrystallization(DRX)and phase transformation(PT)behavior of a wrought β-γ TiAl alloy during hot compression under various deformation temperatures were investigated.The typical work hardening and flow softening features indicated that DRX was the dominating softening mechanism.Both γ-DRX and β-DRX took place during the hot compression.γ-DRX was triggered at all compression temperatures,while the β-DRX was induced when the compression temperature was above 1000 °C.The hot deformation kinetics was calculated,which showed that DRX behavior existed in the whole hot compression process,and the DRX volume fraction increased with the increase of the compression temperature.Combined with the microstructure observation,it concluded that the β/B2+α2→γ PT occurred at 850 °C and 1000 °C,while the γ→β/B2 PT happened at 1050 °C during hot compression,which is important to optimize microstructure.Moreover,the hot compression mechanism changed from dislocation gliding to grain-boundary sliding was discussed.

1.Introduction

Aero-engine materials have to be“stronger and lighter”to withstand the extremely high demanding conditions in the future,which are targeted to reduce weight and fuel consumption as well as significantly decrease CO2emissions [1–6].The realization of this goal should take into account the following two aspects:(1) materials design and (2)structure optimization [7,8].The latter is essential than the former,which involves the relationship among microstructure,process and performance.Generally,γ-TiAl based alloys are widely considered to be one of the most prominent candidates to replace high temperature Tialloys or Ni-based superalloys due to their outstanding mechanical properties such as low density,excellent anti-oxidation and corrosion resistance,high specific stiffness and good creep resistance [9–12].However,γ-TiAl based alloys can scarcely be manufactured by conventional forging due to its intrinsic brittleness [4].Recently,to overcome this limitation,a kind of novel β-solidifying multi-phase TiAl alloy has been developed to form complex components under isothermal conditions by near-conventional forging,owing to a considerable quantity of residual β/B2 phase exist in the microstructure.Correspondingly,the third generation of TiAl based alloys has been developed.A notable example of such an alloy is TNM alloy(Ti-(42–45)Al-(3–5) Nb-(0.1–2) Mo-(0.1–0.2) B [at%]),this alloy has been used in forging low-pressure blades (6–7 level) which has been successfully implemented in PW1100 turbo engine for Airbus A320neo [13].Previous studies showed that disordered β phase is beneficial for hot deformation of TiAl alloy,because the fact that disordered β phase has more independent slip systems [14,15],but the plasticity of TiAl alloy at room temperature was limited by the ordered B2 phase.Therefore,it is necessary to control the microstructure by regulating the content of the β phase.In recent years,many beneficial types of researches about hot compressive deformation of TiAl based alloys have been conducted.Meanwhile,the flow behavior and microstructure evolution characteristic have been expounded[16–18].Studies have focused on the γ phase,ignoring the β/B2 during the deformation.Moreover,another βγ TiAl alloy has been found to show superplastic distortion at higher temperatures with a particular strain rate of 10−4s−1[19,20],which is beneficial to form a complicated component of TiAl alloy.Thereby,it is the importance to investigate the microstructure evolution at a lower strain rate.Moreover,the DRX has a competent time to take place to homogenize microstructure.Meanwhile,phase transformation (PT)behavior is critical to control the fraction of phases during the thermomechanical coupling process [21,22].Compared with the γ-phase,βphase transformation and DRX behavior have a significant influence on the microstructure and mechanical properties of the β-γ TiAl.The objective of the present work is to unveil the underlying DRX and PT behavior of the wrought β-γ TiAl alloy during the hot compression at the strain rate 10−4s−1.The subsequent detailed deformation kineticscurve was calculated to explain the deformation mechanism and DRX behavior.Moreover,the characteristic microstructure observation was analyzed by using the scanning electron microscope (SEM) technique equipped with electron backscatter diffraction (EBSD) in detail.This work contributes to understanding the DRX and PT behavior of wrought β-γ TiAl alloy during the hot compression process,favoring control of the microstructure homogeneousness.

2.Materials and experimental

A cylindrical ingot of TiAl alloy was produced by the triple vacuum arc remelting(VAR)method,followed by hot isostatic pressing(HIP)at 1280 °C for 4 h under the pressure of 140 MPa.The detailed actual chemical composition is given in Table 1.After HIP,the billet with a dimension of Φ203 × 352 mm was packed by Q235 steel and hot forged by three fires at 1170°C,and the diameter of the forged pancake is Φ 420 × 100 mm finally.Fig.1 shows the typical microstructure of the this wrought TiAl alloy.Fig.1(a) shows the SEM image in BSE mode,which shows the initial microstructure mainly constituted equiaxed γ-TiAl phase (black),β/B2 phase (white) and α2-Ti3Al phase(grey).Fig.1(b) shows the phase and grain boundary distribution map based on the EBSD with a step size of 0.2 μm.The state of the microstructure was almost recrystallized,including a few remnant lamellar colonies.The volume fraction of γ,β/B2 and α2phases was about 69%,18.9%,and 12.1%,respectively.The mean grain size was 6 μm approximately.Besides,low angle grain boundaries(LAGB)was measured with a misorientation(θ)of grain boundaries between 2°and 15°(Black line),and the θ of high angle grain boundaries(HAGB)was higher than 15° (Light blue line).The boundaries with 57° ≤θ ≤63° were considered as twin boundaries(TB)(Purple line).The blue bars represent γ grains,yellow bars represent the intergranular α2phase,and red bars represent β/B2 phase as shown in Fig.1(b).

Table 1 Detailed chemical composition of the wrought β-γ TiAl alloy.

The hot compressive specimens with a diameter of 8 mm and a height of 12 mm were cut from the forged pancake by electric-discharge machining,and the compression direction was parallel to the forging direction of the pancake.The hot compression was implemented on a Thermecmastor-Z thermal mechanical simulator at 850 °C,900 °C,950 °C,1000 °C,and 1050 °C respectively with an initial strain rate of 10−4s−1,and the compressive reduction ratio was 60%.Some mica sheets were pasted on the sample surfaces to reduce the friction before compressive deformation.All compression tests were heated using an induction heating system at a given heart rate (10 K/s) from room temperature to compression temperatures,and kept for 300 s to ensure a uniform temperature distribution within the samples.All the compression tests were processed in a vacuum,and the samples were quenched using helium to freeze (~50 K/s) the high temperature microstructure after hot compression.

The microstructure analysis of the samples before and after hot compression sectioned in the center parallel to the compression axis was performed by scanning electron microscopy (SEM) and conducted on a ZEISS Sigma 500 (ZESS Corporation,Germany) equipped with an EBSD system operating at 20 kV.The specimens for EBSD analysis were made by the once mechanical grinding and electropolishing on a Struers Lectropol-5 (Denmark,Struers Corporation) in a solution of 35% n-butyl alcohol,5% perchloric acid and 60 methanol with a voltage 30 V holding 20 s.Additionally,EBSD analytical test was executed with a scan step size of 0.2 μm to obtain the detailed orientation information after compression.The geometrically necessary dislocations(GND) maps from EBSD data were calculated by using the software named HKL Channel 5.

3.Results and discussion

3.1.Flow softening of the β-γ TiAl alloy

Fig.2(a) shows the flow stress-strain curves of wrought TiAl alloy compressed at different temperatures (850 °C–1050 °C) at an initial strain rate(10−4s−1).All flow curves presented a typical“single-peak”flow feature,as shown in Fig.2(a) i.e.the flow curves exhibited work hardening at the initial stage,then with the strain increasing the dynamic softening gradually occurred till steady-state.The peak stress(σp)was obtained after the work hardening,which caused by the formation and accumulation of the dislocations.At the initial stage of the hot compression,the density of dislocations increased significantly.As the hot compression proceeded,DRV occurred first and then formed numerous sub-boundaries.Moreover,the fine sub-structure grew,and DRX happened when the driving force reached a critical value subsequently,which eliminated the dislocations and refined the microstructure [23].Finally,the stress became steady-state (σss) when the equilibrium of work softening and work hardening was obtained.This similar phenomenon also found in other TiAl alloy [17].When compressed at 850 °C or 900 °C,the flow stress exhibited a softening behavior after the peak stress significantly,while the softening rate of the present alloy was lower than the low Al high Nb TiAl alloy[22].As the temperature increased to 950 °C or 1000 °C,the softening rate decreased significantly (see Fig.2(a)).When it is compressed at 1050 °C,the flow stress attained a steady-state after peak stress rapidly.It is generally accepted that DRX phenomenon is natural to be activated in TiAl alloy during hot compression since γ-phase is a low stacking fault energy (SFE) phase,and the DRX is considered to dominate in the softening stage [24].It is worth to note that all the curves reached the steady-state when the true strain reached about 0.7 during the hot deformation.This demonstrates that DRX may be maximized,which is beneficial for microstructure homogeneity during the hot compression.

Fig.1.Typical microstructure of the β-γ TiAl alloy,(a) SEM image in BSE mode,(b) phase and grain boundary distribution map.

Fig.2.(a)Flow curves of the wrought β-γ TiAl alloy after hot compressed at indicated temperatures with a specific strain rate of 10−4 s−1,(b)the activation energy(Q) and stress exponent (n) as a function of deformation temperatures.

Based on the strain-true stress curves,the Arrhenius constitutive relationship among strain rate (ε˙),deformation temperature (T) and flow stress (σ) during the thermal compression process can be established,which could be expressed as the following equation [25,26]:

where A is a material constant,Q is the activation energy,E is Young's modulus,and R is the universal gas constant.

To explain the hot deformation kinetics,both Q and n were calculated from stress-strain curves at different deformation temperatures(see Fig.2(b)) by using the peak stress.To derive the solution at all temperatures,the additional compression tests (at 10−2s−1and 10−3s−1under 1000°C)were conducted to acquire the value of n at 1000°C firstly.The detailed calculation process is shown in previous related research[22],the Q and n can be drawn as the following equation from equation (1):

As Fig.2(b) shows,the value of Q and n changed with the deformation temperature,which indicates the deformation mechanism altered with the increase of the deformation temperature.The stress exponent(n) improved from 2.79 to 1.93 and then increased to 2.49,higher than the low Al high Nb alloy at the same conditions[22],which manifested the hot deformation mechanism is a mixture of grain boundary sliding and dislocation gliding.Besides,it was found that the rate-controlling device was also modified with the increasing of compression temperature.Also,the activation energy is increased firstly and then decreased with the deformation temperature,which is related to the microstructure evolution and phase transformation.The value of Q is more substantial than the self-diffusion activation energy(150 kJ/mol) of β-Ti [27] but smaller than the self-diffusion activation energy(390 kJ/mol) of Al atoms in γ-TiAl alloy [28],which suggests that the deformation mechanism was restricted by lattice diffusion rather than grain boundary diffusion.Furthermore,the value of Q can reflect the ability during deformation generally.Compared with other TiAl alloy like Ti–42 A l–8Nb–(W,B,Y) alloy [29] and Ti-42.5 A l–8Nb-0.2W-0.2B-0.1Y alloy [22],the wrought β-γ TiAl alloy has a lower Q,which suggested that this alloy has excellent hot workability during the hot compression.On the one hand,when the initial state of the alloy was forged,there were lots of dislocations and deformation storage energy for the subsequent DRX.Additionally.There was sufficient time for dislocations motion and subgrains growth at a lower strain rate.Hence,it is speculated that the DRX was activated and responsible for the softening of stress.

3.2.Dynamic recrystallization behavior during the hot deformation

3.2.1.Dynamic recrystallization kinetics

Fig.3.(a) True stress-true strain flow curves at 1000 °C-10−4 s−1 and (b) DRX volume fraction as a function of the strain of the wrought β-γ TiAl alloy hot compressed at different temperatures.

Fig.3(a)shows the true strain-true stress curves of the wrought β-γ TiAl alloy compressed at the condition of 1000 °C-10−4s−1-60%.The curve shows the typical DRX type softening curve,and that the dynamic recovery(DRV)was fragile to be negligible.Therefore,it is necessary to study the DRX behavior during the hot deformation.The calculation of DRX volume fraction (XDRX) could be processed by Ref.[29]:

where XDRXis DRX volume fraction,σ is the true stress,σDRVis the true stress where the only DRV occurs.

Both σDRVandcould be replaced byσpapproximately due to the DRV during the hot deformation process could be ignored as shown in Fig.3(a).Based on Eq.(3),the relationship between XDRXand strain at different temperatures was calculated,as shown in Fig.3(b).It can be seen that the curves are substantially the“S" type curves.The XDRXincreased with the increase of strain until the strain reached about 0.7.Notably,it is remarkable that the XDRXincreased sharply at the initial strain,which suggests that DRX was induced easily in this wrought β-γ TiAl alloys.Moreover,the degree of DRX increased with the deformation temperature at a specific strain,which can be used to predict the DRX behavior and optimize the hot deformation process [30].

3.2.2.γ and β phase dynamic recrystallization

The Kernel Average Misorientation (KAM) is an average difference in orientation between the pixel j and all measurements around the pixel j.The KAM can be expressed as follows [31]:

where K is the number of pixels around the pixel number j (4 in our case)and ωjkthe misorientation angle between pixel couples(j,k).The KAM values (degree) can be used to determine the Geometrically Necessary Dislocation (GND) densities [32].The bigger KAM value,the higher dislocation density,and vice versa.In general,dislocation can be substantially consumed by DRX,and therefore the extent of DRX in a deformed alloy can be evaluated by KAM.

Fig.4 shows phase distribution,GND maps and DRX characteristic of γ and β phase at the different compression temperatures,respectively.Fig.4(a,c,e) shows the phase distribution at the different compression temperatures.When compressed at 850 °C,the γ grains were compressed perpendicular to the compressed direction.Meanwhile,it is evident that a mass of β phase was elongated,and some γ grains were encompassed by the β phase,as shown in Fig.4(a).Correspondingly,much dislocation moved from the inside to boundary,where the GND density is higher,as shown in Fig.4(b).Increasing to 1000 °C,the deformed γ grains were gradually equiaxed,and the elongated β phases were broken and refined,where the DRX may occur(see in Fig.4(c)).DRX of γ and β grains improves the dislocation motion and decreases the GND density (see in Fig.4(d)).However,there also was some high GND density area,where the dislocation was challenging to cross the interface between α2and γ within lamellae,resulting in a dislocation plug [33].When the compression temperature was 1050°C,as shown in Fig.4(e),the lamellae decomposed and grains had equiaxed and uniform significantly,which promoted dislocation movement and disappearance by grain rotation.And the GND density was lower than deformed at lower temperatures (see in Fig.4(f)).

Generally,the microstructure of a deformed alloy can be divided into three types based on the orientation analysis.Fig.4(g and h)shows the fractions of recrystallized grains,the substructure grains and deformed grains of γ and β phase at different compression temperatures,respectively.It can be seen that the volume of γ-DRX and substructure grains increased with the raising of the deformation temperature.Reversely,the deformed grains decreased with the raising of the deformation temperature,as shown in Fig.4(g).Moreover,it can be conducted that the γ-DRX mechanism is DDRX from the changing of DRX and substructure grains.Fig.4(h) shows the fractions of recrystallized grains,the substructure grains and deformed grains of β phase at different compression temperatures.The fraction of β-DRX increased from 24.88% to 94.5% with the increased deformation temperature,which indicates that the β phase was DRXed completely.Correspondingly,the fraction of deformed grains decreased from 68.88% to 1.53%.Because elevated temperature can promote the DRX with more active energy,which is beneficial to nucleation and growth of the deformed β grains [34].

3.3.Microstructure evolution under different deformation temperatures

The microstructures of the deformed specimens at the strain rate of 10−4s−1and different temperatures ranging from 850 °C to 1050 °C are shown in Fig.5.Additionally,the misorientation characteristic of the GB is demonstrated in the EBSD map.Comparing with the initial state,the grain was significantly refined clearly,as shown in Fig.5(a–c)and Fig.6(a).As shown in Fig.5(a),there were lots of DRX grains that surround the residual lamellar colonies and grain boundaries.Moreover,the β/B2 grains and lamellar colonies,were elongated along the direction perpendicular to the compressive direction (see in Fig.5(d))when compressed at 850 °C.Meanwhile,the γ phase recrystallized obviously and numerous γ grains with extremely fine size formed as Fig.6(a)shows.This may be a response to the sharp drop in flow stress after the peak as shown in Fig.2(a),and demonstrates that the hot compression at 850°C was dominated by β/B2-intragranular strain and γ-DRX.

Furthermore,the numerous LAGBs located in the boundary of the γ phase,which indicates that the dislocation moved from the interior of grain to grain boundary during hot deformation.When the temperature increased to 1000 °C,the extent of γ-DRX is increased from 24.77% to 35.33%(see in Fig.4(g)),and the size of γ grains increased obviously as Fig.6(a) shows.The microstructure was more uniform with the mean grain size was about 3 μm,as shown in Figs.5(b) and Fig.6(a).Moreover,the occurrence of β-DRX generated a breakup of the elongated β phase gradually as Fig.5(e) shows,Corresponding to the increase of the fraction of HAGBs in β phase,as shown in Fig.6(b).As mentioned above,DRX generated with the driving force reached a critical value,that is to say,the driving force can satisfy the γ-DRX and β-DRX at 1000°C simultaneously.At the same time,the GND density at 1000°C was reduced and more uniform(see in Fig.4(d)).Nevertheless,there were still a few residual lamellar colonies need to be decomposed(see in Fig.5(b)),where the GND was high.

Promoting the temperature to 1050 °C,the grain of γ-DRX and β-DRX grew obviously,the γ and β/B2 grain were equiaxed with the mean grain size are about 4.5 μm as shown in Fig.5(c,f)and Fig.6(a).The residual lamellar colonies were decomposed completely.This phenomenon also occurs in previous research [18].Meanwhile,the HAGBs almost distributed around the γ and β/B2 grains,as shown in Fig.6(b),which proves that DRX occurred in γ and β/B2 phase completely.Hence,the microstructure of the wrought β-γ TiAl alloy became more uniform as shown in Fig.5(c,f).As shown in Fig.4(f),the GND was minimal at this deformation temperature.

It can be noted that twin boundaries (TBs) existed in the DRXed grains frequently,which may show that the γ-DRX is twin-related DRX[34].Due to the DRX,the mean grain size of the γ phase has a visible change,as shown in Fig.6(a).Besides,few twins formed in the β phase at all chosen deformation temperatures,which resulted from that the bcc β phase has more operative slip systems and lower strength.It can be inferred that the β-DRX mechanism is CDRX.

Fig.4.Phase distribution (a,c,e),GND maps (b,d,f)and DRX characteristic (g,h)of γ and β phase at the different compression temperatures,respectively.(a,b)850 °C,(c,d) 1000 °C and (e,f) 1050 °C.

Furthermore,the misorientation of γ,β/B2 and α2phases was analyzed with increasing compression temperature to illuminate the controlling mechanism during the hot compression process.Fig.6 shows the level of the grain size distribution(GSD)and grain boundary distribution (GBD) (including LAGBs,HAGBs and TBs) of three phases at different compression temperatures.As shown in Fig.6(b),the fraction of HAGBs for γ phase increased from 27.9%to 32.3%and then to 40.87% with the temperature increasing from 850 °C,1000 °C–1050 °C,respectively,which indicates that the γ-DRX may be responsible for the deformation.Furthermore,the fraction of LAGBs for γ phase decreased from 44.45%,41.26%–26.68%with the temperature increased from 850 °C,1000 °C–1050 °C,respectively.Compared with the initial state,the intragranular deformation might be a predominant deformation mechanism at low temperature,which is agreed to the microstructure characteristics.As for β/B2 phase,the tendency of HAGBs and LAGBs was similar to the γ phase during the hot deformation,which shows that the β phase had the same effect on hot deformation.Furthermore,the β/B2 phase was softer than the γ phase at elevated temperature,which is beneficial for the hot deformation.The fraction of TBs of γ phase increased from 2.08% to 9.25% as the compression temperature increased from 850°C to 1050°C,as Fig.6(b)shows.Most of the γ-DRX grains were twin-related to the original grains,while the other grain boundaries are HAGBs from EBSD images(see in Fig.5(d),(e),(f)).This phenomenon indicates that twinning is related to γ-DRX feature in the deformation process.As shown in Fig.6(a),the grain size of the α2phase decreased slightly compared to the initial state at different compression temperature.There is no change of LAGBs of α2phase,while the HAGBs of α2phase changed slightly.This may result from the rotation of impendent γ-grains and β/B2-grains.This indicates that the α2phase underwent a grain break slightly without recrystallization Corresponding to the microstructure characteristic as Fig.5 shows.In a word,it is helpful for γ-DRX and β-DRX process as the deformation temperature arising.

Fig.5.EBSD maps of the wrought β-γ TiAl alloy hot compressed at different temperatures(a,d)850°C,(b,e)1000°C(c,f)1050°C.(a,b,c)band contrast maps,(d,e,f) phases map overlapped with grain boundaries.

3.4.Phase transformation at different deformation temperatures

Fig.6.GSD and GBD of γ phase,β/B2 phase and α2 phase measured in Corresponding EBSD maps before and after hot compression at indicated temperatures.(a)GSD (b) GBD.

Fig.7.Fraction of different phases (β,γ,α2) at indicated temperatures.

In particular,it is found that the phase fraction changed with the compression temperature (see Fig.7),which indicates the phase transformation (PT) during the hot compression.It can be observed from Fig.7 that the fraction of β and α2phase at 1050 °C decreased from 18.9% to 17.2% and 12.1%–9.83%,respectively,while the fraction of γ phase increased from 68.5%to 73.3%compressed at 850°C or 1000 °C.This suggests that the β/B2+α2→γ PT occurred at 850 °C or 1000 °C objectively.Furthermore,it is noted that the α2phase always appeared with the β phase and the γ phase embed into β phase,as shown in Fig.5(d and e).This phenomenon also suggests that the β/B2+α2→γ PT occurred.Therefore,the PT is decisive in the increase of activation energy (Q) before 1000 °C.When the alloy was compressed at 1050°C,the PT behavior was also found.Nevertheless,it is different from the compression at 850 °C or 1000 °C.i.e.the fraction of β increased significantly from 18.9% to 21.8%and γ phase decreased from 12.1% to 10.3%,while the fraction ofα2phase virtually unchanged,which indicates that the γ→β/B2 PT occurred at high compression temperature.Therefore,the Q decreased at 1050 °C as shown in Fig.2(b).In summary,PT behavior plays an essential role in hot compression.

It is noted that the residual lamellar colonies were decomposed during the hot deformation,scilicet,the α2→β/B2 PT occurs [18].Inversely,the fraction of β/B2 phase decreased at 850 °C and 1000 °C,which suggests that there existed another PT to occur at this compression temperature.When it was compressed at 1050°C,the residual lamellar colonies were decomposed entirely,the α2→β/B2 PT occurred.Nevertheless,it was observed that this transformation was induced within recrystallized grains.

As mentioned above,the β/B2+α2→γ and γ→β/B2 PT were detected by the orientation analyze in EBSD map.It is known that the lamellar microstructure forms from parent α phase abide by the Blackburn orientation relationship (OR)({0001}α//{111}γ,<11–20>α//<110>γ) for TiAl alloy during solidification[35].Fig.8 shows the part of EBSD and inverse pole figures (IPF)images at 850 °C and 1050 °C.According to Fig.8,the β+α2→γ PT occurred when the wrought TiAl alloy was compressed at 850 °C(numbers 1,2,3 and 4 represent α2,γ (new),β and γ phase,respectively),the misorientation was analyzed among them as shown in Fig.8(a) and Corresponding pole figures Fig.8(c).It is found that the new γ phase (2) and α2phase (1) followed the Blackburn OR,and the Kurdjumov-Sachs (K–S) OR ({110}β//{111} γ,<111>β//<110>γ)[36]was detected between the new γ phase(2)and β phase(3)as the red ring shows.The new γ phase located in the hug of α2and β phase.However,the orientation relationship was not detected among the initial γ phase(4),α2(1)and β phase(3).This suggests that the new γ phase was induced from adjacent α2and β phase.Besides,many fine γ grains that located in the middle of α2and β phase were detected,as shown in Fig.8(b),which demonstrates that the β+α2→γ PT occurred during the compressed deformation at 850 °C.Furthermore,the deviation was calculated to explain the possibility of PT.The orientation variations between γ and α2phase,β and γ phase were about 3.46°and 10.61°,respectively.These values of the deviation are less than the angles of LAGBs,indicating that the β+α2to γ PT occurred quickly.However,considering that the divergence between β and γ phase was closed to a standard K–S OR,this may result from the fact that PT and plastic deformation,as well as interaction,simultaneously were induced during the hot compression process.

When the deformation temperature rose up to 1050°C,the γ→β/B2 PT occurred during the hot compression process as mentioned above.As Fig.8(b) and Corresponding pole figures shows that the fine β grain(6) was surrounded by the original γ phase (5) and (7).Besides,the presence of Kurdjumov-Sachs (K–S) OR [37] ({111}γ//{110}β,<110>γ//<111>β) was detected between original γ grains (5),(7) and β grains (6) as shown in Fig.8(f) and Table 2.Also,the deviation between β (6) and γ (5),(7) phase was about 2.59° and 3.09°,less than the angles of LAGBs,which demonstrates that the γ→β/B2 PT occurred.As we all know,the γ phase is harder than the β phase at high temperature,which is the reason for the decrease of Q with increasing β phase content.

Table 2 Orientation relationship among the new γ,α2 and β grains at different compression temperatures.

4.Conclusions

The DRX and PT behavior of wrought β-γ TiAl alloy during the hot compression has been investigated via the SEM and EBSD.γ-DRX and β-DRX expression behaviors have been analyzed,and PT in recrystallized grain discussed in detail.

(1) The true stress-strain curves exhibit typical work hardening and flowing softening features.The value of activation energy Q changes with the deformation temperature which is resulting from the phase transformation.The lower Q value indicates better hot workability of the β-γ alloy.

Fig.8.Drawing of partial enlargement from Fig.5(b) and (f).(a,c) IPF map,(b,d) phase map,(e,f) Pole figures.

(2) The extent of DRX increases with an increase in hot deformation temperature.Also,the“S" type relationship between DRX volume fraction and hot deformation temperatures has been obtained to optimize the process.Both γ-DRX and β-DRX occurs during the hot compression.γ-DRX is triggered at all compression temperatures,but the β-DRX is induced when the compression temperature above 1000 °C,and the former is the main reason for flow softening.

(3) The phase transformation of β/B2+α2→γ occurs at 850 °C and 1000°C,while the phase transformation of γ→β/B2 occurs at 1050°C during hot compression,which is essential to the hot deformation of the wrought β-γ TiAl alloy during a relatively lower strain rate 10−4s−1.

(4) Hot compression mechanism of the wrought β-γ TiAl alloy changes with temperatures.The dominant deformation mechanism is dislocation gliding at 850 °C and 1000 °C.Nevertheless,the deformation mechanism is grain-boundary sliding at 1050 °C.

Declaration of competing interest

The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper.

Acknowledgements

This work was financially supported by the Aeronautical Science Foundation of China (No.201936053001),the National Natural Science Foundation of China (No.51771150),the Natural Science Foundation of Shaanxi Province(2018JM5174) and the Research Fund of the State Key Laboratory of Solidification Processing,NPU),China(Grant No.2019-TS-07).