Hot deformation behaviors of WE71 alloy under plain strain compression at elevated temperature
2020-07-29BangqiYinXiangyiXueBinTangYiWangHongchaoKouJinshanLi
Bangqi Yin,Xiangyi Xue,Bin Tang,Yi Wang,Hongchao Kou,Jinshan Li
State Key Laboratory of Solidification Processing,Northwestern Polytechnical University,Xi'an,710072,China
Keywords:WE71 alloy Hot deformation behavior Dynamic recrystallization Shear band Plain strain compression
ABSTRACT Hot deformation behaviors of WE71(Mg–7Y-1Nd-0.5Zr)alloy was investigated by plain strain compression tests conducted at temperatures ranging from 350°C to 500°C and strain rates varying from 0.01 s-1 to 10 s-1.Results show that the hot deformation of WE71 was accompanied by the precipitation of rich Zr phase with granular shape and block-shaped phase rich in element Y.When deformed at low temperature and high strain rate,the softening behavior of the alloy was synergically determined by shear bands propagation,adiabatic heating,twinning formation and dynamic recrystallization(DRX).For the conditions of high temperature and high strain rate,DRX was the major softening mechanism while the formation and annihilation of extension twinning resulted in a special flow curve characteristic at the strain of around 0.3.According to the microstructural observations,it can be concluded that the irregular flow curves of WE71 alloy during plain strain compression process are mainly ascribed to shear bands propagation,adiabatic heating,twinning formation and DRX.
1.Introduction
As the important light metal structural materials,the magnesium alloys have opened new horizons for developing commercial alloys with successful use in a wide variety of applications [1–3].However,due to their hexagonal close packed (HCP) crystal structure and the limited slip systems in cold and warm deformation conditions,typical wrought magnesium alloys exhibit poor formability at low temperatures,thus limiting their processing and widespread use in industrial production[4,5].At elevated temperature,the formability performance of the alloy can be improved as a result of grain refining and stress softening behavior caused by the activation of more dislocation slips and dynamic recrystallization (DRX) [6].As a kind of Mg–Y-Nd based magnesium alloys,WE71 (Mg–7Y-1Nd-0.5Zr,wt%) possesses remarkable aging hardening effect and good thermal stability,it has good application prospects at the condition of high temperature [7–9].
In order to get a better understanding of the hot-deformation behavior of WE71 magnesium alloys,the flow characteristics of the asReceived alloy at high temperature should be researched.During the hot deformation processing,dynamic recrystallization (DRX) is an important softening mechanism.Studies have shown that continuous dynamic recrystallization (CDRX) and discontinuous dynamic recrystallization (DDRX) may occur during the process of hot deformation,resulting in grain refining and a softening behavior in the flow curves [10–13].Another important softening mechanism during the hot deformation of magnesium alloys is shear bands propagation and adiabatic heating.A large amount of literatures reported that shear bands should be produced during compression of magnesium alloys when deformed at low temperature and high strain rate[14–16].Some researchers [17,18] believed that the shear bands propagation and adiabatic heating would cause a great softening behavior during hot deformation.Cheng et al.[19] assumed that the flow curves characterized by“double peaks”during plain strain compression are mainly ascribed to the synergy effect of shear band propagation and adiabatic heating.An important feature of magnesium alloys is the twinning produced during hot deformation [20].Liu et al.[21] thought that the formation of extension twinning would bring about grain reorientations during deformation process,resulting in a great flow softening.As is discussed above,the reason that cause the softening behavior of magnesium alloys during hot deformation could be DRX,shear band propagation or deformation twinning.
Besides,the precipitation of second phase should make some difference on the flow behavior of magnesium alloys.Hantzsche et al.[22]found that the formation of precipitate caused pinning effects within grain boundary,thus hindering the movement of grain boundary.Robson et al.[23]reported that large particles(>1 μm diameter)were able to stimulate the recrystallization behavior of magnesium alloys deformed in plane strain compression.Asqardoust et al.[24] believed that the dynamic precipitation of precipitates during hot deformation of WE54 alloy was accompanied with the depletion of strong strengthener from the matrix while the precipitation phase was characterized by weak strengthening effect.Thus,the role of precipitates on the hardening behaviors of the alloy could be neglected.
Although large amounts of literatures have investigated the flow behaviors of magnesium alloy during hot deformation,few researches have been done on the flow curve characteristics and the Corresponding deformation mechanism of Mg–Y-Nd based magnesium alloy under plain strain compression.The aim of this work is to investigate the flow curve characteristics of WE71 magnesium alloy under plain strain compression at elevated temperatures.Particularly,the deformation mechanism of the alloy deformed at 450 °C/10s-1and 500 °C/10s-1were systematic discussed.Besides,the precipitates of the alloy were investigated by EDS spectrum and SEM observations.
2.Experimental procedures
The initial WE71 alloy was provided by Aerospace research institute of materials and processing technology.The nominal composition of the as Received alloy was Mg–7Y-1Nd-0.5Zr (wt%).The rectangular samples of 10 × 15 × 20 mm3were used for plane strain compression at 350,400,450 and 500 °C,with strain rates of 0.01,0.1,1 and 10s-1,respectively on the Gleeble-3500 thermal mechanical simulator.The specimens were maintained at the target temperatures for 3 min with a heating rate of 9 °C/s,and then they were deformed to a true strain of
0.8.After that,the deformed samples were quenched immediately to reserve the high temperature deformed microstructure.
For microstructural observations,the deformed samples were sectioned along the direction parallel to the compression axis.All the samples were prepared by standard grinding procedures and etched by the solution of 4 vol% nitric acid in alcohol.The microstructures evolutions were observed by an optical microscopy (OM) and a scanning electron microscopy (SEM) equipped with an energy dispersive X-ray spectroscope(EDS).The phase compositions were obtained from the Xray diffraction (XRD) analysis using Cu-Ka radiation over 2θ=10–90°at 3°/min.For the electron backscattered diffraction (EBSD) observations,the samples were electropolished using a solution of 5% perchloric acid+95%methanol at a voltage of 3 V for 60 s.The deformed samples were observed by an EBSD system operating at 20 kV,equipped with OIM analysis software.The TEM observation was carried out on a Talos F200× TEM at voltage of 200 kV.
3.Results and discussion
3.1.Initial microstructure and precipitated phases of WE71 alloy
As shown in Fig.1(a),the initial microstructure of the material was characterized by equiaxed microstructure with deformation flow lines.Besides,fine precipitates were found distributed within the grain.From Fig.1(b),a large number of fine recrystallized grains were found in the initial microstructure with random orientation.The XRD results shown in Fig.1(c) indicate that the WE71 alloy mainly consisted of α-Mg matrix,Zr particles,Mg24Y5and Mg41Nd5phases.
In order to explore the real composition and distribution of precipitations,the alloy was detected by SEM and EDS techniques (displayed in Fig.2).From Fig.2(b)–(e),it can be observed that two kinds of second-phase precipitations existed in the microstructure.The square phase demonstrated in Fig.2(b) was rich in Y element,and the coarse particle phases shown in Fig.2(c) were mainly rich in Zr element.As shown in Fig.2(a),the square particles randomly distributed,while the coarse particles were mainly distributed along the deformation flow lines.Besides,there were many fine precipitates along the flow lines,which were rich of Nd and Y.Literatures[8,9]have found that Mg41Y5and Mg24Y5eutectic phases existed at the grain boundary of as cast sample.After compression deformation,Mg41Y5and Mg24Y5eutectic phases would redistribute along the compression flow lines.According to the XRD patten denoted in Fig.1(c),the fine precipitates were mainly Mg24Y5and Mg41Nd5phases.During the hot deformation process,these precipitations may have important effects on the hardening behavior of the alloy.The detailed information is discussed later.
The TEM image and the selected area electron diffraction (SAED)pattern of the square phase of the deformed alloy are exhibited in Fig.2(f)–(g).The SAED pattern of the square phase indicates that the structure of the square phase was face-centered cubic structure (f.c.c.),and the lattice constant a was 0.54 nm (Fig.2(g)).
3.2.Characteristics of flow curves
Fig.3 shows the stress–strain curves of the deformed alloy at different temperatures and strain rates.As we know,the flow stress is closely related to strain rate as well as deformation temperature.When deformed at 350 °C/1s-1,350 °C/10s-1and 400 °C/10s-1,the curves for the samples were terminated at relatively low strain levels,indicating the premature shear fracture of the samples.Apart from these cases,the specimens showed a higher deformability and an ultimate strain of~0.8 was finally achieved.
With the increasing of deformation temperatures and decreasing of strain rates,the flow stress and peak stress decreased obviously.Particularly,when deformed at 450°C and 500°C with strain rate of 10 s-1,the flow curves were of great difference from those deformed at other strain rates.This phenomenon has rarely been seen in other studies.In general situations,the flow stress increases rapidly to a peak value followed by a gradually decrease to a steady state when work hardening and dynamic softening reach a balance,which is the typical characteristics of DRX curves.While in this paper,the flow stress experienced a rapid drop after it reached the peak stress.This may be attributed to shear band propagation and adiabatic heating.Besides,the curves exhibited secondary and tertiary hardening behavior,which may be due to the formation of precipitations and the entanglement of dislocation.The detailed explanation will be discussed later.

Fig.1.Microstructure of the as-Received WE71 alloy:(a) SEM microscopy;(b) EBSD derived IPF map;(c) XRD pattern.

Fig.2.Second-phase particles in the WE71 alloy:(a)SEM image of flow lines and block-shaped phases;(b)SEM image of block-shaped phases;(c)SEM image of flow lines;(d) EDS spectrum of point A;(e) EDS spectrum of point B;(f) TEM bright-field image and (g) SAED pattern of square phase.

Fig.3.Flow curves of WE71 alloy at different deformation conditions:(a) 350 °C;(b) 400 °C;(c) 450 °C;(d) 500 °C.

Fig.4.Flow curve of WE71 alloy deformed to various strains at 450 °C/10s-1.

Fig.5.EBSD derived IPF maps and Corresponding IQ maps of WE71 alloy deformed at 450 °C/10s-1 to a strain of:(a,d) 0.3;(b,e) 0.4;(c,f) 0.5.
3.3.Flow curve analysis and microstructure evolution at 450 °C/10s-1
The flow curve and Corresponding microstructure evolution of WE71 alloy deformed at 450 °C/10s-1are displayed as Fig.4.The results show that the flow stress reached a peak value followed by a sharp decreasing trend.The flow softening behavior was closely related to various special microstructure characteristics such as shear bands propagation,twinning formation,dynamic recrystallization (DRX) and dynamic recovery (DRV).
The tree opened up so that Mr. Coyote could go inside to rest, then it closed to keep him safe. Mr. Coyote slept for hours. When he woke up he could not remember what he had said to make the tree open. He said, Let me out Mr. Tree , but nothing happened. He said, Please let me out now!
As we all know,DRX plays an important role in the softening behavior of magnesium alloy[25].To investigate the influence of DRX on the softening behavior of the as-Received alloy,the inverse pole figure(IPF) maps of the alloy deformed at different strains are exhibited in Fig.5.The IPF maps superimposed with grain boundaries reveal the grain distributions and recrystallization situations of the deformed materials.With the increase of strain,the initial grains were gradually elongated along the direction around 45° away from the compression direction,and more and more fine DRX grains appeared at the bulged grain boundaries,which is an important factor causing the softening behavior.However,the amount of DRX grains is not enough to cause the great softening behavior.

Fig.6.Flow curve of WE71 magnesium alloy deformed to various strains at 500 °C/10s-1.

Fig.7.EBSD derived IPF maps and Corresponding IQ maps of WE71 magnesium alloy with the deformation condition of 500°C/10 s-1 at the strains of:(a,e)0.2;(b,f) 0.3;(c,g) 0.5;(d,h) 0.7.
It is assumed that shear bands propagation should be another reason resulting in this great softening behavior.From the optical micrograph it was clearly seen that the shear band with“S”shape was throughout the entire sample at the strain of around 0.5.The previous studies show that the“S”type shear bands are mainly due to the synergic effect of adiabatic heating,deforming and distributing of instantaneous friction[26,27].During the deformation process,the stress concentration occurs in an“X”type region of the specimen.The“X”type stress concentration is supposed to be related to surface tension of the specimen and the friction during deformation,which significantly promotes the occurrence of shear band due to the favorable orientation.Due to the difference of deformation-induced heating and the nonuniform of instantaneous friction,one of the two branches becomes stronger,weakening the second branch.With further deformation,the interaction of adiabatic heating and strain,together with the increasing of interfacial friction,promotes the propagation of the stronger branch,thus forming the“S”type shear bands.With the strain increasing from 0.3 to 0.5,the shear band propagated along one diagonal of the longitudinal section.Within the shear band,the intense deformation resulted in the adiabatic heat rises within the alloy,causing a great softening behavior during the process.Therefore,the softening behavior at this stage can be explained by shear bands propagation and adiabatic heating.
Apart from the shear bands propagation and adiabatic heating,the deformation induced twinning is another important factor causing the great softening behavior at the strains ranging from 0.3 to 0.5.At the initial stage of deformation,there was almost none twinning existed in the alloy.When the alloy is deformed to a strain of 0.4,there was about 8.12% {10–12} extension twinning (as denoted in Fig.5(e)) formed in the initial grains of the alloy.Through the formation of extension twinning,the basal planes were reoriented from a hard slip to a softer direction,thus causing a great increase in Schmid factor and resulting a great flow softening as denoted in the flow curve as denoted Fig.4.When the strain was up to 0.5,the extension twinning almost disappeared in the image quality(IQ)maps of the alloy.The formation and annihilation of extension twins should be the important reason to result in this particular flow curve characteristic of WE71 alloy deformed at 450 °C/10s-1.

Fig.8.SEM images of WE71 alloy deformed with the condition of 500°C/10 s-1 at the strains of:(a) 0.2;(b) 0.3;(c) 0.5;(d) 0.7.
Based on the analysis above,it can be concluded that the shear band propagation,the extension twinning along with DRX result in the great softening behavior during the plain strain compression,while the shear band propagation and extension twinning play a major role.After the strain reached around 0.5,the shear bands with“S”shape passed totally through the entire width of the sample,and the extension twinning almost disappeared.At this stage,the flow softening behavior is mainly due to dynamic recrystallization,while precipitations and work hardening may be the cause of the hardening behavior.Besides,the highdensity dislocation within the shear bands leads to dislocation strainfield interaction that hinders the motion of dislocation,resulting in a hardening behavior in the shear band[28].The weakening of softening behavior at the strain of around 0.5 can be mainly explained by the transformation of softening mechanism from shear bands propagation and extension twinning to DRX.
3.4.Flow curve analysis and microstructure evolution at 500 °C/10s-1
When deformed at 500 °C/10s-1,the flow curve was characterized by a great softening behavior along with secondary and tertiary hardening behavior,which was of great difference from that deformed at 450 °C/10s-1.As shown in Fig.6,with the increase of strain,the flow stress experienced a greater decrease after it reached a peak stress compared with that deformed at a lower strain rate.An important reason is dynamic recrystallization (DRX).To investigate how the DRX influences the flow behavior of the alloy deformed at 500°C/10s-1,the IPF maps and the Corresponding IQ maps of the samples deformed at different strains are exhibited in Fig.7.It's not hard to find that the initial grains were elongated along the direction perpendicular to the compression direction with the increasing of the strain.Besides,there were more and more small size equiaxed grains to appear,indicating that the accumulation of strain promotes the occurrence of dynamic recrystallization.Due to the influence of dynamic recrystallization,there is a tendency to decrease in flow stress with the increasing strain(as seen in Fig.6).
After further EBSD analysis and a large number of literature researches,we have found that the precipitation of second phases is not the main reason resulting in the curve characteristic at the strain of around 0.3.In the WE71 alloy,both Y and Nd are strong solid solution strengtheners.During the hot deformation process,the precipitation of second phases may cause the decrease of strong strengthener from the matrix.At the same time,while strengthening effect attributed by the precipitation phase is small[24].Therefore,the precipitation of second phases is unable to bring about a great hardening behavior.Although it can be seen from Fig.8 that the fraction of precipitates first increased and then decreased,the variation of the precipitates was neglected on the whole during the deformation process.Thus,it is not under consideration when analyzing the hardening mechanism.
In this paper,the variation of the curve deformed at 500°C/10s-1to a strain of 0.3 is mainly ascribed to the formation and annihilation of extension twins during deformation process.During the hot deformation process,extension twinning was initiated in the earliest stages of deformation.When the strain was increasing to 0.2,a large number of twins(8.12%)(as shown in Fig.7(e))formed in the initial grains.After the strain was up to 0.3,the extension twinning was almost invisible(as shown in Fig.7(f)).The formation and annihilation of extension twins caused this particular curve characteristic at the strain of around 0.3,as is denoted in Fig.6.
4.Conclusions
The hot deformation behavior of the Received WE71 magnesium alloy has been investigated by means of plane strain compression in the temperature range of 900–1050°C and strain rate range of 0.01–10 s-1.
(1) Two kinds of precipitations have been found during the hot deformation of WE71 alloy,including particle-shaped phase rich in Zr and block-shaped phase rich in Y.The precipitations play a limited role in the hardening behaviors of the alloy during the plain strain compression,which is hardly reflected in the flow curves.
(2) For the WE71 alloy compressed at the deformation condition of 450 °C/10s-1,the flow curve is characterized by a sharp decrease after it reaches peak stress.This great softening behavior is mainly ascribed to the great temperature rises caused by the adiabatic process of shear bands propagation as well as the formation of extension twinning.
(3) When the alloy is deformed at the deformation condition of 500°C/10s-1,the flow curve is of great difference from that deformed at 450 °C/10s-1.During the whole deformation process,the major reason of its softening behavior is dynamic recrystallization (DRX).The special flow curve characteristic at the strain of around 0.3 is mainly attributed to the formation and annihilation of extension twinning.
Declaration of competing interest
The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper.
Acknowledgments
This work was financially supported by the Natural Science Foundation of Shaanxi Province(2018JM5174),and the Research Fund of the State Key Laboratory of Solidification Processing,NPU),China(Grant No.2019-TS-07).The authors would like to thank the Shaanxi Materials Analysis and Research Center for TEM testing.
杂志排行
Progress in Natural Science:Materials International的其它文章
- Compositional complexity dependence of dislocation density and mechanical properties in high entropy alloy systems
- Construction of Ni–Al–Ru EAM potential and application in misfit dislocation system
- Microstructure and heat treatment for Ni3Al-based single crystal alloy with different crystal orientations
- Dynamic recrystallization and phase transformation behavior of a wrought β-γ TiAl alloy during hot compression
- Role of β(FeAl) nanoparticles in abnormal grain growth in the annealing of cast Cu-Al-Mn-Fe shape memory alloys
- 3D printed titanium scaffolds with ordered TiO2 nanotubular surface and mesoporous bioactive glass for bone repair