某油田集油干线弯管开裂失效原因研究
2020-03-18许艳艳葛鹏莉高多龙
许艳艳 葛鹏莉 高多龙
摘 要:通过对某油田集油干线弯管刺漏部位的化学材质分析、微观形貌观察和残余应力分析,結果表明:该管段材质的金相组织、硬度和强度不满足相应标准要求,导致管材的脆性增加,致使在缺陷位置发生裂纹起源,在局部拉伸应力、疲劳载荷及残余应力影响下,管段在裂纹处快速撕裂。
关 键 词:集油干线;开裂;材质缺陷;应力
中图分类号:TQ 052 文献标识码: A 文章编号: 1671-0460(2020)02-0497-04
Abstract: The chemical composition of puncture site of the elbow of the main oil gathering line in an oil field was analyzed, its micromorphology was observed, and its residual stress was analyzed. The results showed that the metallographic structure, hardness and strength of the pipe segment materials did not meet the requirements of the corresponding standards, resulting in the increase of the brittleness of the pipe, causing the crack origin at the defect location. Under the influence of local tensile stress, fatigue load and residual stress, the pipe segment rapid tore at crack.
Key words: oil gathering main line; crack; material defect; stress
某油田集油干线于2013年10月18日投产使用,管长6.93 km。管线设计压力等级4 MPa,管材为L245NS,规格为?168 mm×5 mm,介质流向发生改变的位置采用无缝热煨弯管。管道内部为油气水混输介质。管道运行压力为0.5 MPa,运行温度为75 ℃。管内介质为油、气,含有少量的水,地层水分析结果中呈弱酸性,pH值在5.13~7.02之间,Cl-含量约2 984~29 516 mg/L,硫化氢含量在107.36~633.53 mg/m3之间。管道内壁采用无溶剂液体双组分环氧涂层防护。管道外壁采用30 mm厚聚氨酯泡沫聚乙烯夹克防腐保温。弯管规格为φ168×6.0-R900,L245NS,R=6D,热煨弯管,热煨工艺依据标准SY/T5257-2012《油气输送用钢制弯管》。2016年2月,该管线的弯管发生刺漏,带来一定的经济损失和环境影响。本文通过断口形貌观察、弯管材料性能测试等检测手段,分析了弯管失效的原因,为采取有效的预防性措施提供依据。
1 管段宏观形貌观察
取样管段如图1所示。弯管圆周长为530 mm,管道外壁裂纹长度为415 mm,管道内壁裂纹长度为410 mm,开裂处距离左端焊缝处为210 mm。由于管道外壁裂纹的长度大于管道内壁裂纹长度,且裂纹的剪切唇为后期快速断裂形成,因此判断裂纹源自图1(b)所示的平滑区域。……