炼油厂重催装置换热器管束的泄漏原因
2017-10-11王晓军朱文胜
王晓军,石 荣,朱文胜,缪 磊
失效分析
炼油厂重催装置换热器管束的泄漏原因
王晓军1,石 荣1,朱文胜2,缪 磊2
(1.兰州理工大学材料科学与工程学院,兰州730050;2.中国石油天然气集团公司兰州石油化工公司,兰州730060)
某炼油厂重催装置E203换热器在运行过程中发生了管束泄漏,采用光学显微镜、扫描电镜、以及能谱分析等方法对失效原因进行了分析。结果表明:换热管内表面发生了严重的点蚀,腐蚀产物主要有Fe(OH)3、FeS和FeCl2;换热管内表面腐蚀产物中含有腐蚀性离子(Cl-和S2-),这是导致管束腐蚀失效的主要原因。
换热管;腐蚀产物;腐蚀失效
Abstract:Leaking of tubes within heat exchanger of residue fluid catalytic cracking unit in an oil refinery occurred during running.The failure reasons were analyzed by means of optical microscopy,scanning electron microscopy and energy disperse spectroscopy.The results show that serious pitting occurred in the inner surface of the tube,and the corrosion products mainly consisted of Fe(OH)3,FeS and FeCl2,corrosive ions such as Cl-and S2-in the heat exchange tubes were the main reason for the corrosion and failure of tubes.
Key words:heat exchanger tube;corrosion product;corrosion failure
某炼油厂运行中的一台140万吨/年重油催化裂化装置油气-热水管壳式换热器(E203)的管束在使用15个月后发生泄漏,致使设备无法正常使用,影响生产。为查明原因,避免类似事故发生,对失效件进行了失效分析。
换热器管板采用16MnR钢,管束采用20号钢渗铝,尺寸为φ19 mm×2.0 mm。换热器操作参数见表1。由表1可见,壳程的温度、压力均较管程的高,表明壳程167℃高温的油气换热给管程123℃的水。观察发现泄漏发生在管束外壁,此处壳程介质为含污水的油气。对换热器壳程内污水水质进行分析,p H为8.96,呈碱性,总溶解固体1 714 mg/L,wNa+130.8 mg/L,wCl-298.8 mg/L,wS2-145.3 mg/L,wHCO3-78.1 mg/L,污水中Cl-和S2-等对碳钢腐蚀起加速作用的有害离子含量很高。

表1 换热器参数Tab.1 Parameters of heat exchanger
1 理化检验
1.1 外观检验
经停机抽取管束检验,发现换热器外表面腐蚀严重甚至已发生穿孔现象。用砂轮机切取管束中发生泄漏的一处弯管,将管道沿轴向剖开后的内外壁形貌见图1。……