隧道喷射混凝土浸出物对工程排水水质的影响规律
2025-08-11罗鹤松孟凡强龚勋李传松代勁松王东梅龚正君
中图分类号:X703.1 文献标志码:A 文章编号:2096-6717(2025)04-0226-08
Influence of leaching substances from tunnel shotcrete on water quality
LUO Hesong L1 ,MENG Fanqiang1,GONG Xun1,LI Chuansong 2 ,DAI Jinsong², WANG Dongmei',GONG Zhengjun1 (1.Schoolof Environmental Science and Enginering,Southwest Jiaotong University,Chengdu611756,P.R.China; 2. China Railway Eryuan Engineering Group Co.,Ltd.,Chengdu 6loo31,P.R. China)
Abstract:Water-sewage diversion of tunnel construction drainage is an important engineering technique to reduce tunnel construction sewage discharge.However,the leaching substances of unstable tunnel shotcrete can affect the drainage water quality. Therefore,the study of the influence of leaching substances on the water quality during the stabilization process of shotcrete is of great significance for the precise implementation of wastewater separation technology.The static and dynamic experimental methods have been applied to the systematic study ofthe polltion indicators and leaching laws of shotcrete.The static experimental results show that when water comes into contact with newly poured concrete,the large release of alkaline substances can lead to a rapid increase in the pH of the water, becoming an important pollution factor affcting the water quality. The dynamic experimental results show that the curing time of concrete,the ratio of water to concrete (the volume-to-volume ratio of water sample to concrete, L/S ),and the contact area between concrete and water all affect the water quality.When the curing time of the concrete is less than three days,the calcium hydroxide crystal inside theconcrete is not solidified by the C-S-H gel,which is easy to continue to precipitate,leading to the pH of the contact water sample exceeding the standard. With the increase of curing time,the leaching alkaline substances decrease significantly. When the maintenance time reaches 28 days,the pH of the leaching solutiondrops below 9,which can meet the requirements of comprehensive wastewater discharge.When the L/S (2号 ratio is low,the leaching substance has a significant impact on the pHand alkalinity of the water sample.When the L/S ratio exceeds 40:1 , the leaching substance has no significant impact on the water quality of the water sample.The larger the contact area between the concrete and water samples,the easier itis foralkalis in the concrete to dissolve and precipitate,and the more significant the impact on the pH and alkalinity of the water quality.
Keywords: drainage; separation of clean and dirty water; shotcrete; leaching substances; tunnel construction
隧道施工是道路建设中对周围地表水影响最大的活动之一[1],特别是当隧道建设位于环境敏感地区时,隧道开挖、衬砌、灌浆等施工过程中会产生大量废水,这些废水直接排放可能会造成严重的环境问题。目前,隧道施工废水主要采用物理沉降等方式处理后排放,但在隧道施工场地受限的情况下,施工废水会因沉降时间不足导致悬浮物超标排放。针对此问题,有学者提出隧道施工排水“清污分流\"技术[3-5],即在洞内两侧设置临时侧沟,收集掌子面、初支段及二衬段的线状水和股状涌水,作为清水直接排放,掘进过程中产生的排水则利用中心排水沟收集,进人污水站处理后排放。实际工程中,掌子面和初支段的涌水在隧道水压较小时沿侧壁流至侧沟,二衬段盲管涌水也会与隧道衬砌材料发生接触,隧道内喷射的混凝土在与隧道涌水接触时产生的浸出物质会对水质产生一定影响。
未稳定的混凝土接触隧道涌水会导致水体pH值迅速升高[6],Setunge等[7对养护 24h 的混凝土浸出试验结果表明,水体的pH值在 12h 内升至11.5。王家庆等8使用复合降碱工艺处理生态混凝土,然后进行浸出试验,发现浸出液的pH值仍达到11以上。此外,水泥生产过程中使用的初级和次级原料中锌、铬、铜、钙、镁、钾、钠等元素在未稳定的混凝土中也可能被水体浸出[9。因此,隧道涌水流经未稳定的喷射混凝土时,浸出物质会影响工程排水水质,对受纳水体的水质构成威胁[10]……p>