Causes of the formation of pit defects on the surface of the enamel layer
2020-10-13,
,
Research Institute,Baoshan Iron & Steel Co.,Ltd.,Shanghai 201999,China
Abstract: During the production of the inner walls of ovens,pit defects were formed on the surface of the enamel layer that was enameled on the cold-rolled steel via electrostatic powder spraying and sintering.The paper elaborates on the microstructure and element distribution of the enamel-steel interface and the enamel layer.Optical microscopy,scanning electron microscopy,and energy-dispersive spectroscopy were adopted to investigate the microstructure of a longitudinal section of the defect,and the pit-forming causes were analyzed.The results show that rusty spots lead to pit defects.During high-temperature firing,there is an inadequate fusion and reaction between iron oxides of the rusty spots and the enamel glaze.The rusty spots are closely related to pretreatment process;thus,to avoid their occurrence,electrostatic powder spraying and sintering should be performed timely after forming,degreasing,and thorough drying of the metal sheets.
Key words: cold-rolled steel for enameling; pit defects; rusty spots; pretreatment process before enameling
1 Introduction
Enameled steel is a type of composite material con-sisting of a steel plate and enamel powder,between which strong chemical bonds form after high-temperature burning[1-3].Enameled steel has the toughness and impact resistance of a steel plate;it is anticorrosive,abrasion-resistant,nonflammable,easy to clean as well as radiationless and has aesthetics of an inorganic enamel layer[4-5].Enameled steel has been favored by the majority of users due to its comprehensive performance.With the continuous development of production techniques and pro-cessing equipment,enameled steel has increasingly been used in more fields,including lighting,home appliances,metallurgy,chemical engineering,and architecture[6-7].
The quality of enameled products depends on the steel plate,enamel glaze,and enameling tech-nique[8-10].The steel plates should have stable mechan-ical properties,such as strength and formability,and favorable enameling performance,such as resistance to fish-scale and pinhole defects and good adherence.Furthermore,the pretreatment process and enameling technique should be tightly con-trolled by downstream users.It is well known that pro-per pretreatment is very important,otherwise enameled products will have various enameling defects.The steel plates will have maximum cleanliness and roughness after proper pretreatment,which will provide favorable conditions for smoothly enameling[11].
In this paper,white-dot defects were formed on the surface of the enamel layer that was electrostatic powder-sprayed and sintered on cold-rolled steel.Optical microscopy (OM),scanning electron micro-scopy (SEM),and energy-dispersive spectroscopy (EDS) were adopted to detect and analyze the white-dot defects,and then the causes for their occurrence were analyzed.
2 Observation of defects
The cold-rolled steel for enameling was delivered with oiled surface to be used for making inner walls of ovens.The manufacturing flow was as follows:
Cutting→Forming→Spray-type degreasing→Rinsing→Drying→Electrostatic powder spraying→Sintering→Inspecting.
Firstly,the plate surface was degreased by spraying,rinsed,and dried.After the pretreatment,the plate was electrostatic powder-sprayed with enamel and sintered.However,white-dot defects occurred on the enamel layer surface of the inner walls of ovens,as shown in Fig.1.The magnified photograph demonstrates that the diameters of the pit defects are approximately 600-800 μm,which are much larger than those of the pinhole defects.The surface of the pit is dark gray,which contrasts from the normal enamel layer surface,and unevenly granular.To define the causes for the formation of the pit defects,relevant analyses were carried out.
3 Discussion on the causes for defect for-mation
Fig.2 shows an SEM micrograph of the pit defects.EDS was also adopted to analyze a pit defect and the enamel layer.It can be seen that the pit defect contains elements such as C,O,Na,Si,and Fe,and among those,the peaks of Fe and O stand out.On the other hand,the enamel layer contains elements such as C,O,Na,Al,and Si,which are normally found in electrostatic powder.Through comparison,it was found that the main difference between the pit defect and enamel layer was the existence of Fe.The causes of pit defect formation need further investigation.
A metallographic specimen was cut along the longitudinal section from the steel plate near the pit defects.The defect in the enamel layer was revealed after mechanical grinding,but the metallic matrix was not exposed completely.After that,the metal-lographic specimen was polished and etched in 4% nital for investigation via OM and SEM.
3.1 Investigation and analysis of non-defective enamel layer microstructure
The microstructures observed by OM and SEM are shown in Fig.3.As can be seen in Fig.3(a),small,uniformly distributed bubbles are present in the non-defective enamel layer.The thickness of the non-defec-tive enamel layer is approximately 120 μm.Fig.3(b) shows that the interface between the metallic matrix and the enamel layer is uneven,and there is a thin transition layer between them,which improves adherence.
3.2 Investigation and analysis of the microstru-cture of a defective enamel layer
Fig.4 shows the microstructure of the defective enamel layer investigated via OM and SEM.As seen in Fig.4(a),the bubbles are distributed unevenly and have different sizes in the defective enamel layer.The size of an individual bubble reaches 110 μm.Large bubbles break through the enamel layer,forming pinhole defects on its surface;thus,they will reduce corrosion resistance of the enameled steel.Fig.4(b) shows that there are two types of abnormal microstructure alongside the metallic matrix and non-defective enamel layer.The first one is a layer of light gray abnormal microstructure at the interface of the metallic matrix and the enamel layer,extending to the metallic matrix.The second one is a layer of light gray abnormal microstructure near the surface of the enamel layer.
To confirm the causes of the defects,an energy spectrum analysis was carried out by EDS.EDS spectrum 1 shows that the non-defective enamel layer contains C,O,F,Si,K,Ca,Na,and other elements,which coincide with the components of regular electrostatic powder.EDS spectrum 2 shows the abnormal microstructure at the interface of the metallic matrix and the enamel layer contains Fe,O,C,Si,and other elements,which shows that there are no main components of enamel,except for iron oxides and SiO2,in the abnormal microstructure.By inference,the iron oxides come from the steel plate before spraying and result from rust spots on the surface of the steel plate based on their shapes.From measurement,the rust spot has a diameter of 0.5-1.0 mm.In the processing of high-temperature firing,complicated chemical reactions occur between rust spots and enamel powder.The chemical reactions shown in Equations (1)-(4) firstly occur on the sur-face in a short period of time,because rust spots have a certain thickness.The reminder of the rust spot cannot participate in the reactions completely.Gases such as O2,CO,CO2,and H2are generated by the above reactions and form small bubbles in the enamel layer.The gas pressure gradually increases,and small bubbles continue to emerge and grow as the chemical reactions proceed.When the gas pressure exceeds the strength of the enamel layer,the gas will break through the enamel layer and pit defects with a diameter of 600-800 μm will form on the surface.The same abnormal microstructure as shown in spectrum 3 is detected close to the surface of the enamel layer,caused by less resistance to gas diffusion of the enamel compared to that of the metallic matrix during the process of high-temperature firing.
Through the above analysis,it is inferred that pit defects are caused by rust spots.During the process of high-temperature firing,iron oxides in the rust spots and enamel melt have not fully fused and reacted,thus,there is abnormal microstructure left at the rust spots,which is different from the enamel layer after high-temperature firing.
4 Defect prevention measures
Based on the production process of the inner walls of ovens,the causes of the rust spots on the surface of steel sheets are as follows:
(1) The oil film breaks due to the decrease in surface tension where there was significant deformation induced by the stamping process of steel sheets,accelerating rusting of the surface of a steel sheet.
(2) The surface of a steel sheet is oil-free after degreasing,leading to quick rusting.
(3) A thin film of water will be absorbed on the surface of a steel sheet,when the steel sheet is dried incompletely after being washed or the air is moist,which causes it to rust easily.H+ions attract electrons and form hydrogen molecules if the water film is strongly acidic,which is called the hydrogen evolution corrosion.More oxygen will be dissolved,if the water film is weakly acidic or neutral,and O2will attract electrons to form OH-groups,which is called the oxygen absorption corrosion.The oxygen absorption corrosion is the main cause of steel rust.
Therefore,every stage during the manufacturing process of enameled products should be strictly controlled.Electrostatic powder spraying should be carried out timely after the steel sheet is formed,degreased,and dried completely.
5 Conclusions
(1) White-dot defects on the surface of the enamel layer of the inner walls of ovens are caused by rust spots on the surface of the steel sheet before electrostatic spraying.
(2) During high-temperature firing,iron oxides in the rust spots and enamel melt fuse and react,but the reactions are insufficient.Thus,the enamel layer at rust spots contains Fe,O,C,Si,and other elements,which differ from the components of the regular enamel layer.A large volume of gases such as O2,CO,CO2,and H2is generated during firing.When the gas pressure exceeds the strength of the enamel layer,the enamel layer will rupture,forming pit defects on its surface.
(3) The inner walls of ovens are fabricated via a long manufacturing process,so the cause of rust spots is not unique.Thus,additional processing must be performed after a steel sheet is formed,degreased and dried completely.Once corrosion occurs,electrostatic spraying and firing should not be allowed.
杂志排行
Baosteel Technical Research的其它文章
- Influence of sulfur on inclusion and pitting resistance of 316L stainless steel
- Mechanical and corrosion properties of N08825 CRA clad pipeline steel
- Research on material design and high-temperature friction and wear properties of new graphitic steel
- Bottom dross defect and its transformation behavior during the galvannealing process
- Theoretical study on the torque values of premium connections