Research on material design and high-temperature friction and wear properties of new graphitic steel

2020-10-13,

Baosteel Technical Research 2020年3期

,

Research Institute,Baoshan Iron & Steel Co.,Ltd.,Shanghai 201999,China

Abstract: To solve the problem of the severe mismatch between the product and roll materials in the preliminary rolling line,a new graphitic steel material was designed,its microstructure and high-temperature friction and wear properties were investigated.Moreover,the feasibility of replacing semi-steel with this new material in the V1 stand roll was studied herein.The results show that the graphitic steel matrix is strengthened by silicon and nickel elements.The presence of spherical graphite also provides self-lubrication and heat conduction and prevents the propagation of cracks.Carbides in the appropriate amount and size strengthen the matrix,reduce the cracking effect of the matrix,and are not easily broken,thereby reducing high-temperature abrasive wear.Under the same high-temperature friction and wear conditions,compared with semi-steel,the wear-scar surface of graphitic steel exhibits less wear-scar depth and wear volume,a smaller friction coefficient,reduced oxide layer thickness,and fewer instances of peeling and microcracks.Therefore,the newly designed graphitic steel has higher wear resistance and hot-crack resistance than semi-steel,which makes it feasible for use in replacing semi-steel as a new V1 frame roll material in the blooming mill.

Key words: graphitic steel; microstructure; high-temperature friction and wear properties; high-temperature tensile strength; thermal cracking resistance

1 Introduction

In the preliminary rolling unit,large steel ingots are rolled into cylindrical rods and square billets.The preliminary rolling process also provides blanks for engine crankshafts and oil well pipes,reopens large continuous casting slabs,and improves the quality of finished products[1].With the higher demand by downstream users regarding the mechanical prop-erties of products,the product structure of the preliminary rolling unit has changed from simple to multiple specifications and the product category has changed from carbon steel to carbon steel in combination with alloy steel[2].However,the V1 stand roll used in preliminary rolling has always been made from semi-steel material.During its use,problems such as thermal cracks,fractures,roll-surface bulges,and high roll consumption are prone to occur,which directly affect product quality,production quality and consumption costs.The serious mismatch between the product and roll materials and the equipment capabilities in the preliminary rolling line has become an urgent problem that must be resolved.

Graphitic steel is a new material whose charac-teristics fall somewhere between those of ductile iron and semi-steel,having the properties of both steel and iron[3- 4].Due to the deeper V-groove,severe working conditions,large rolling force,and total amount of rolling steel used in the preliminary rolling V1 frame,hot-crack resistance,wear resistance,and strength are the main roll performance indicators.As yet,there are no reports on the use of graphitic steel as a V1 stand roll material.

In this paper,with regard to the problems of roll surface cracks and bulges,fractures,and high roll consumption,and the working conditions of the preliminary rolling V1 stand using semi-steel rolls,a graphitic-steel material for use in the V1 stand roll was designed,and its composition,microstructure,and high-temperature friction properties were investigated to improve its thermal-crack and wear resistance.

2 Experimental method

Based on the working conditions of the preliminary rolling V1 stand,the composition,micro-structure,and mechanical properties of the graphitic steel were designed.The raw materials were melted in a 500 kg vacuum induction furnace,and cast into alloy ingotsφ300 in size,followed by heat treatment and machining into samples with the desired specifications.The room-temperature and high-temperature hardness values were determined using an AHR-150P automatic-touch-screen digital Rock-well hardness tester and a DAKOMASTER 300 high-temperature hardness tester,respectively.The microstructures of the samples were observed using a Zeiss LSM800 confocal microscope and scanning electron microscopy.The high-temperature tensile test was conducted using a Gleeble 3500 instrument.An Rtec MFT-5000 friction tester was used to perform a ball-disk-type high-temperature friction and wear test,using an alumina ball as the upper sample and the study sample as the lower sample.The test temperature was set to 600 ℃ with a load of 30 N,a rotation speed of 3 000 rpm,a rotation radius of 15 mm,and test time of 15 min.

3 Results and discussion

The composition,microstructure,and mechanical properties of the prepared graphitic steel were examined,tested,and compared with those of the semi-steel used in the preliminary rolling V1 stand.The wear mechanisms of the two were considered and possibility of using graphitic steel as a preliminary rolling V1 stand roll material was investigated.

3.1 Material design

Strictly controlling the chemical composition of molten steel,optimizing the nodularization and inoculation process,controlling the roundness of the graphitic balls and the content,morphology,and distribution of carbides,and reducing the dissevering degree of the substrate are the basis for ensuring the high strength,toughness,and wear resistance of graphitic steel.

Table 1 shows the designed and measured com-position values of the graphitic-steel roll material and Table 2 shows the chemical composition of the semi-steel roll material.

Table 1 Chemical composition of the graphitic-steel rolls %

Table 2 Chemical composition of the semi-steel rolls %

3.2 Design of heat treatment process

In the design of the heat treatment process,hardness,strength,toughness,and higher wear resistance were taken into consideration,as was the thermal cracking resistance[5].The heat treatment process used in this paper was as follows.The preheat treatment started with annealing at 980 ℃ for 2 h,then slowly cooling to 600 ℃ in the furnace,followed by air cooling.After this preheat treatment,a microstructure comprising ferrite+pearlite+carbide+graphite was obtained.The final heat treatment involved normalizing at 950 ℃ for 30 min,cooling to below 300 ℃ in the furnace with nitrogen protection at a cooling rate of 1.2 K/s,followed by air cooling to room temperature.The tempering process involved heating to 630 ℃ for 120 min,cooling to below 200 ℃ in the furnace,and then air cooling to room temperature.This tempering process was repeated two or three times.After the final heat treatment,a sorbite/spheroidized pearlite matrix structure was obtained,in which the dispersion of pearlite was increased,the structure was refined,and the strength,hardness,and wear resistance were improved in the graphitic-steel rolls.

3.3 Microstructure research

Fig.1 shows a typical microstructure and graphite and carbide rating charts of the graphitic steel.As shown in Fig.1(a),the metallurgical structure of the graphitic steel was fine flake pearlite,spherical graphite,bulk eutectic carbide,and needle-like secondary carbide.The pearlite sheet was so thin that the original austenite grain boundaries can be observed.Carbides were present mainly in the form of granular secondary carbides and very few eutectic carbides.As can be seen from Figs.1(b) and (c),the graphitic-steel microstructure was composed of graphite with grade-3 nodulization and grade-8 size,and carbides with grade-2 carburization.

Fig.2 shows the microstructure of the semi-steel,which can be seen to consist of pearlite and secondary carbides.After casting and solidification,the direction of the pearlite sheet in one grain was consistent.Due to the forging effect,the morphology of the carbide changed from radial to dispersed,and the pearlite layer became irregular.

3.4 Analysis of mechanical properties at room temperature and high temperature

As both the graphitic steel and semi-steel were used as V1 stand materials in the preliminary rolling,their working conditions and room-tem-perature hardness values (HSD) were equivalent,i.e.,about 48.The room-temperature hardness was obtained via a certain heat treatment process.As shown in Fig.3,as the temperature increased,the hardness values of the graphitic steel and semi-steel gradually decreased.When the temperature was increased from 100 to 700 ℃,the hardness (HR30N) of the graphitic steel decreased from 50.3 to 23.5,and the hardness of the semi-steel decreased from 36.8 to 0.The results show that the high-temperature hardness values of the graphitic steel at different temperatures were higher than those of the semi-steel.

Table 3 shows the tensile and impact properties of the graphitic steel and semi-steel at room temperature.It can be seen that the yield strength(Rp0.2) of the graphitic steel and semi-steel was 602 and 464 MPa,the tensile strength (Rm)was 680 and 940 MPa,the section elongation (A) was 1.1% and 6.0%,the section contraction rates (Z) were 1.0% and 6.5%,and the impact energies (AkU2) were 5.5 and 5.0 J,respectively.These results indicate that the yield strength and impact energy of the graphitic steel are higher than those of the semi-steel,but its tensile strength,section elongation,and section contraction rate are all lower than those of the semi-steel.

Fig.4 shows the high-temperature tensile strength of the graphitic steel and semi-steel.It can be seen that when the temperature was 900 ℃,the high-temperature tensile strength of the graphitic steel was 253.7 MPa,which is lower than that of the semi-steel.However,the high-temperature tensile strength of the graphitic steel and semi-steel at 1 000 ℃ was basically the same,i.e.,175.7 and 175.1 MPa,respectively.

3.5 High-temperature friction and wear perform-ance

Table 4 shows the high-temperature friction and wear performance parameters of the graphitic steel and semi-steel.

Table 3 Room-temperature tensile and impact properties of the graphitic steel and semi-steel

Table 4 High-temperature friction and wear performance parameters

Figs.5(a) and (b) show two-dimensional (2D) images of the high-temperature wear morphologies of the graphitic steel and semi-steel,respectively.It can be observed that the width of the wear scar of the graphitic steel was slightly bigger than that of the semi-steel,but its depth was shallower.Micro-cutting,pear groove,flaky spalling,and compacted rolling of the spalling can be observed on the wear-scar surface of both the graphitic steel and semi-steel.At the same time,there were many micro-cracks on the wear surfaces,which was due to the generation and downward extension of fatigue microcracks.There was less flaky spalling on the surface of the graphitic-steel wear scar than on that of the semi-steel.

Figs.6(a) and (b) show three-dimensional (3D) illustrations of the high-temperature friction and wear-scar surfaces of the graphitic steel and semi-steel,respectively,in which the depth and morphologies of the wear scars can be observed.The macroscopic morphologies of the two clearly indicate that the depth of the wear scar on the graphitic steel was significantly shallower than that of the semi-steel.

Fig.7 shows the high-temperature wear friction coefficient curves of the graphitic steel and semi-steel.As shown in Fig.7(a),the friction coefficient of the graphitic steel increased slightly at the beginning of the wear test,and the friction coefficient fluctuated between 0.15 and 0.28.In Fig.7(b),it can be seen that the friction coefficient of the semi-steel increased slightly with the increase of wear time,fluctuating between 0.20 and 0.48.This indicates that the friction coefficient of the graphitic steel was more stable than that of the semi-steel.

As shown in Table 5,the width,depth,and volume of the wear scar of the graphitic steel were 1 720 μm,9.50 μm,and 6.78×10-3mm3,respectively,and those of the semi-steel were 1 600 μm,22.73 μm and 4.23×10-2mm3,respectively.It is therefore obvious that the wear volume of the semi-steel was greater than that of the graphitic steel,which means its wear resistance was worse than that of the graphitic steel.

Table 5 Quantitative measurements of wear scars

3.6 Discussion of mechanisms of friction and wear

Fig.8 shows the microstructures of the high-temperature wear surfaces of the graphitic steel and semi-steel.It can be seen in Fig.8(a) that there were many microcracks and a few spalling blocks on the high-temperature wear surface of the graphitic steel.However,no microcracks had yet propagated to form spalling.In Fig.8(b),micro-cracks and large-scale abrasion peeling can be observed on the high-temperature wear surface of the semi-steel,as well as a large number of abrasion particles scattered in the spalling pit.

Fig.9 shows the cross-section morphologies of the high-temperature wear scars of the graphitic steel and semi-steel,in which no obvious micro-structural deformation layer can be observed.This indicates that both the graphitic steel and semi-steel had high hardness and strength.Moreover,a few fine cracks can be observed in the cross-section morphology of the wear scar of the graphitic steel,whereas there were more cracks and their subsurface extension depth was greater than the wear scars observed in the cross-section morphology of the semi-steel.This finding indicates that under the same wear force and fatigue conditions,the semi-steel is prone to produce more and deeper microcracks.

To study the oxidation and oxygen element distri-bution conditions,EDS analysis was performed on the graphitic steel and semi-steel wear-scar cross sections.As shown in Figs.10(a) and (b),the oxygen ele-ments extended along the microcracks to the subsurface layer,forming a thin oxide layer on the wear-scar cross section of the graphitic steel.However,as can be observed in Figs.10(c) and (d),on the high-temperature wear-scar cross section of the semi-steel,there were a large number of microcracks that extended deeper into the subsurface layer.Accord-ingly,the oxidation layer of the semi-steel was thicker than that of the graphitic steel,indicating that the oxidation and thermal cracking resistance of the graphitic steel were higher than those of the semi-steel.

According to the comprehensive analyses presented in Figs.8-10,the high-temperature friction and wear mechanisms of the graphitic steel and semi-steel were mainly fatigue wear,abrasive wear,and oxidative wear in varying degrees.

The differences in the high-temperature friction and wear performance of the graphitic steel and semi-steel were closely related to their composition and microstructures.In terms of composition,the carbon content of the graphitic steel was equivalent to that of the semi-steel,its silicon and nickel contents were slightly higher than those of the semi-steel,but its chromium content was lower than that of the semi-steel.The differences in the structures of the graphitic steel and semi-steel were mainly the strengthened graphitic-steel matrix due to the silicon and nickel elements and the lesser dispersion of less coarse secondary carbides and more granular carbides than those in the semi-steel,due to the formation of graphite.

Studies have shown that the morphology,size,and quantity of graphite used in a substrate had important effects on its abrasion resistance and thermal-crack resistance[6-7].Zhang et al.[8]found cluster-like graphite to weaken any dissevering of the matrixes of high-nickel-chromium indefinite-chill cast iron rolls,buffer the thermal and mechanical stresses,and inhibit crack propagation.With an increase in the graphite content,the crack initiation temperature gradually increased,and the initial-crack depth gradually decreased.In their investigation of the Ni/graphite composite coating,Zeng[9]and Wang et al.[10]found that when the graphite content was low,its role in the matrix was not obvious,but as the graphite content increased,the graphite became more dispersed and tightly integrated with the matrix metal.A uniform distri-bution near the grain boundaries was found to increase the dislocation density in the coating,thereby pinning and strengthening the coating.When the graphite content was excessive,however,the graphite was found to disperse on the surface of the coating as a simple substance that had low strength and hardness,which decreased the hardness and wear resistance of the composite.

In this study,the appropriate amount of round graphite was obtained by optimizing the graphite spheroidization and inoculation processes,which played a dual role in the matrix.In terms of wear resistance,a certain amount of graphite in the graphitic steel was found to improve the wear resistance and thermal-crack resistance of the matrix.It is obvious in Fig.7 that at the initial stage of wear,the friction coefficients of both the graphitic steel and semi-steel rapidly increased,and then the wear became stable.During the wear stage,the friction coefficient of the graphitic steel exhibited good stability.This is because the hexagonal layered crystal structure of the graphite tightly binds together the carbon atoms in the same layer,which cannot easily be broken.However,slipping under shear force tended to occur due to the small distance between the atom layers and the weak bonding force.As the wear test continued,the graphite was gradually exposed on the surface and began to adsorb water molecules from the air to form a film,which served to lubricate and protect the friction surface,thereby effectively reducing and stabilizing the friction coefficient,reducing the adhesion and plow wear between metals,and improving the overall wear resistance.This is also the reason why there were fewer exfoliated blocks on the wear-scar surface of the graphitic steel,as observed in Figs.5 and 8.However,an excessive amount of graphite would dissever and reduce the strength of the matrix,thereby increasing the likelihood of deformation and breakage of the graphite edges,which would reduce the effective pressure-bearing surface area,and be detrimental to the wear resistance.This conclusion is consistent with those reported in the literatures[11-12].

With respect to the hot-cracking resistance,during the initial stage of thermal fatigue,microcracks originated from the micro-tips of the spheroidal graphite edges due to thermal stress.Cracks that generated in other parts of matrix or carbides expanded along the grain boundaries or carbides.When these cracks expanded to the graphite,due to the good thermal conductivity of the graphite,the stress caused by the temperature difference was reduced,the crack propagation path zigzagged,the crack tips were passivated,and crack propagation to the depth of the matrix was hindered to a certain extent.Meanwhile,the presence of graphite balls served a similar function to that of circular cavities,which can prevent cracks from expanding and thereby delay and reduce spalling.This indicates that the graphite had the effect of relaxing the stress,which is also an important factor in the graphitic steel having higher wear resistance than the semi-steel.

There were carbides in both the graphitic steel and semi-steel,but the number and sizes of the car-bides in the graphitic steel were smaller than those in the semi-steel.Some studies have shown that the morphology,size,and distribution of carbides had an important influence on the wear and hot-cracking resistance of the materials[13-14].

Xie[15]reported that in low-alloy wear-resistant cast iron under repeated impact,stress tended to concentrate at the interface between carbides that had a continuous network morphology and the matrix,which caused cracking and peeling off.Car-bides with a massive morphology were beneficial to the continuity of the matrix,buffering the stress concentration,hindering the initiation and diffusion of fatigue cracks,and reducing the tendency of peeling off and weight loss.Meanwhile,a dispersion of carbides in a matrix with higher hardness has been found to protect the matrix from wear and improve the wear resistance.Xiong et al.[16]reported that with an increase in the wear load,smaller carbides would peel off from a matrix,whereas larger carbides fragmented first and then peeled off from the matrix.This demonstrates that only when the matrix had carbides of appropriate distribution and size at the same time could wear resistance be improved.Wu et al.[17]reported that the hardness and quantity of carbides had an important influence on the wear resistance of a matrix.With an increase in the carbide content,the hardness of the matrix is increased,which improves the wear resistance.Thus,an appropriate amount of carbides can strengthen the matrix.The larger the volume percentage of carbides,the more easily cracks are generated at the carbide-matrix interface.The more concentrated the carbides,the shorter the crack propagation path,and the stronger the cutting effect on the matrix,which decrease its impact toughness and wear resistance.

The graphitic steel and semi-steel have the same carbon contents and different wear resistance because the total carbide content of the graphitic steel is lower than that of the semi-steel due to the formation of the graphite.In the microstructure of the graphitic steel,it can be seen that carbide particles that are small in size and uniformly dispersed act not only as hard points for strengthening the matrix,but also protrude during the wear process and support the matrix,which effectively reduces the contact area and pressure between the matrix and the abrasive,resists foreign hard particles from pressing into the matrix,and blocks the furrow produced by shear stress.This is the reason why there were fewer furrows and less peeling off on the graphitic-steel wear-scar surfaces in this study,as shown in Figs.5 and 8.

However,in the semi-steel,there was a certain amount of large primary eutectic carbides.During the wear process,these carbides would break and form third-phase particles that aggravated the abrasive wear of the semi-steel.This finding is consistent with the research of Ren et al.[18].

You and I can identify with that little boy. We have scars, too. No, not from an alligator, or anything quite so dramatic. But, the scars of a painful past. Some of those scars are unsightly and have caused us deep regret.

In addition to graphite and carbide,the oxidation resistance of the matrix itself and the synergistic effect of the matrix and hard particles also have a great impact on the wear resistance and hot-cracking resistance of the materials[19-20].In this study,the carbide particles in the graphitic steel were of the appropriate size and were closely incorporated with the matrix.When the carbide particles were squeezed and plowed by the abrasive particles,the surrounding matrix was able to effectively prevent these carbide particles from sliding and spalling by generating dislocation jogs.Because of the good synergy between the matrix and carbides,the graphitic steel exhibited good high-temperature wear resistance.At the same time,the presence of the graphite particles played an effective part in heat conduction and enhanced the thermal stability of the matrix.

As shown in Fig.3,the high-temperature hardness of the graphitic steel was higher than that of the semi-steel,which indicates that the matrix and carbides had better synergy than the semi-steel during the high-temperature wear process.Therefore,as shown in Fig.10,the number and depth of microcracks extending from the wear-scar surface to the subsurface layer and the oxide layer thickness in the high-temperature wear-scar cross section of the graphitic steel were both smaller than those of the semi-steel.With no graphite in the semi-steel,hot cracks can easily generate and extend into the subsurface layer,causing the entry of oxygen molecules into the matrix,which results in a thicker oxide layer.

In summary,in the newly designed graphitic-steel material,carbides of the appropriate amount and size,which do not easily fracture during the high-temperature wear process,can strengthen the matrix and reduce the dissevering effect on the matrix and the degree of abrasive wear.In addition,the presence of spherical graphite in the matrix further hinders crack propagation,while also promoting self-lubrication and heat conduction,which makes its wear and heat-crack resistance higher than those of the semi-steel.Therefore,the newly designed graphitic steel is found to be a feasible replacement for the semi-steel as a new roll material for the V1 stand of the blooming mill.

4 Conclusions

Based on the rolling conditions of the preliminary rolling V1 stand,a new graphitic-steel material with high strength,toughness,and wear resistance was obtained by strictly controlling the chemical composition of the liquid steel,optimizing the spheroidization and inoculation processes,and controlling the roundness of the graphite balls and the content,shape,and distribution of the carbides.

(1) Regarding its composition,the carbon con-tent of the designed graphitic steel was equivalent to that of the semi-steel,but the silicon and nickel contents were slightly higher and the chromium content was lower.The graphitic-steel microstruc-ture was characterized by the formation of the graphite,a lower content of carbides composed of less coarse secondary carbides and a majority of dispersed granular carbides,and a matrix strength-ened by silicon and nickel elements.

(3) Carbides of the appropriate amount and size were dispersed in and strengthened the newly designed graphitic-steel matrix,which reduced the dissevering effect,number of fractures,and abrasive wear.At the same time,in the newly designed graphitic steel,the presence of spherical graphite was found to hinder further crack growth and facilitate self-lubrication and heat conduction to realize higher wear and heat-crack resistance,as compared with those of the semi-steel.Therefore,it is feasible to use the newly designed graphitic steel to replace the semi-steel as the primary rolling V1 stand material.