APP下载

Mechanical and corrosion properties of N08825 CRA clad pipeline steel

2020-10-13,

Baosteel Technical Research 2020年3期

,

Research Institute,Baoshan Iron & Steel Co.,Ltd.,Shanghai 201999,China

Abstract: Corrosion-resistant-alloy (CRA) clad steel combines the good mechanical properties of the base material and the excellent corrosion resistance of the cladding material,while also being much more economical than solid CRAs.As gas and oil fields can have high concentrations of H2S,Cl-,CO2,and other chemicals,the pipes used to transport gas or oil must have high corrosion resistance and good mechanical properties.UNS N08825 nickel-based alloys with their excellent corrosion resistance can be a good cladding material in clad steel.In this paper,UNS N08825+X65 clad steel was produced by two different processes.The thermomechanical and quenching and tempering processes were investigated and their mechanical properties and corrosion resistance were compared.Intergranular corrosion and pitting corrosion tests were conducted and the results were evaluated.A high-pressure and high-temperature gas-field environment was also simulated to test the stress corrosion cracking of the steel.The results show that both clad plates have good mechanical properties and excellent corrosion resistance.The experimental results were compared and the differences between the two processes were identified and discussed.

Key words: clad steel; TMCP; quenching; tempering; pipeline; corrosion; mechanical properties

1 Introduction

With the development of the chemical and petro-leum industries,materials with excellent corrosion resistance and high allowable-working-stress levels are in high demand for the design of chemical vessels and pipes.For their excellent corrosion resis-tance and chloride-ion stress corrosion resistance in petroleum and chemical applications,nickel-based alloys have proven to be a good choice[1].How-ever,due to the low yield strength and high cost of nickel-based alloys,as well as China’s limited domestic production capacity,nickel-based alloys are not an economical option.Another potential option is carbon steels,the strength ranges of which can be adjusted widely and which can easily meet the strength requirements of pipes or pressure vessels.However,the serious drawback of carbon steel is that it tends to have very poor corrosion resis-tance.In some extreme circumstances,the service life of carbon steel can be shortened to just a couple of months when the actual corrosion environment is more severe than expected.Thus,both pure nickel-based alloys and pure carbon steels have critical material defects.Corrosion-resistant-alloy (CRA) clad steel,which combines the good mechanical properties of the base material and the excellent cor-rosion resistance of the cladding material,is becoming the preferred choice of users in the chemical and petroleum industries[2-3].

The oil and gas in some crude oil or gas fields contain high concentrations of sulfur and acid,which require pipeline materials with high corrosion resis-tance.Generally,nickel-based alloys such as UNS N08825 (hereinafter referred to as 825) and UNS N06625 are used due to their excellent corrosion resistance in these circumstances.Due to the high cost and low yield strength of nickel-based alloys,they are typically used as cladding materials in clad plates.In pipes that do not require strong bonding between the liner/cladding and base material,the mechanical lining method may be preferred due to its low cost.However,if high bonding strength is required,metallurgical bonding methods are recom-mended.In the production of the nickel-based alloy clad steel,examples of metallurgical bonding methods include overlay welding,explosive bonding,and hot-rolled bonding.However,the efficiency of overlay welding is relatively low,and its poor surface quality may negatively impact the corrosion resis-tance.The explosive bonding method,due to its pro-cessing limitations,can yield some local unbonded areas that weaken the weld joints and bring the possibility of pipe failure during use.In contrast,hot-roll-bonded clad steel yields a 100% bonding rate with high bonding strength.Therefore,its popularity has gradually grown such that it is now preferred by an increasing number of customers.

In hot-roll-bonded nickel-based-alloy clad steel,there are significant differences in the physical pro-perties of the nickel-based alloy (cladding mater-ial) and the carbon steel (base material).For example,there is a significant difference between the flow stresses of these two materials and between their thermal expansion coefficients.Furthermore,in practical application,there are strict requirements for both the mechanical properties and corrosion resistance of clad steel.In this paper,two different processing routes,thermomechanical processing (TM) and quenching and tempering (Q-T),are presented and their results are analyzed to determine which process is more appropriate for clad-steel applications.

2 Materials and experiments

Nickel-based alloy 825 and pipeline carbon steel were selected as the respective cladding and base materials,respectively.The materials were cleaned and the edges were sealed to produce a vacuum system between the cladding and base materials,which is referred to as a clad slab assembly.Usually,to prevent possible distortion by the dif-ferent flow stresses of the cladding and base materials during hot rolling,a symmetrical double-layer clad slab assembly was used.

The clad slab assemblies were reheated in a furnace to obtain homogeneous composition of the cladding and base materials.Next,two different processing routes were used to study the different properties of the resulting clad steels.In the Q-T process,a clad slab assembly was first hot rolled to produce clad plates,which were then reheated to the solution-treatment temperature,and then the plates were quenched and tempered.In the TM process,a clad slab assembly was thermomechanically pro-cessed to obtain clad plates.

The cladding material 825 alloy was produced on the special-steel production line of Baosteel,the composition of which is shown in Table 1.This com-position is considered to be moderate and conforms to ASTM B424.

Table 1 Composition of 825 cladding material %

Two different low-carbon microalloyed steels were designed to achieve a balance of strength and tough-ness,as shown in Table 2.In addition,small amounts of alloying elements such as Ti,Nb,V,Ni,Cu and Mo were added to obtain grain refinement,precipitation strengthening,and solid-solution strengthening.The contents of the carbon steel were in accordance with API 5L in sour environments.

The thickness of the 825 clad plates produced using the Q-T and TM processes was 20 mm in total,with 3 mm for the cladding material and 17 mm for the base material.Since clad plates are used in oil and gas fields,a series of strict evaluations must be made according to the general requirements of the gas and oil transport environments.Here,the mechan-ical properties,intergranular corrosion,pitting corrosion,and stress corrosion cracking of the 825 clad-steel plates were investigated.

Table 2 Main alloy elements and carbon equivalent (Ceq) levels in carbon steels%

3 Results and discussion

3.1 Mechanical properties

The tensile tests were conducted only on the base materials according to the ASTM A265 standard as the cladding materials are not considered in the calculations of the strength of the materials.Similarly,a Charpy V notch (CVN) test and a drop weight tear test (DWTT) were performed only on the base materials.

Table 3 shows a comparison of the tensile results for the Q-T and TM processes,in which the yield strength and tensile strength of the clad steels manufactured using the Q-T and TM processes both meet the requirements for X65-grade steel in accordance with API 5L for alloy design.

Table 3 Strength of clad steel 825+X65

Table 4 shows the results of the CVN test and DWTT,which reveal that the Q-T process can be used to achieve the required toughness in a moderate-temperature environment.The average upper-shelf energy is 275 J,which is lower than the 413 J of TM-treated clad steel.The DWTT results show that the clad steel produced by the Q-T pro-cess may qualify for use in pipes that require good toughness at temperatures that do not fall below -20 ℃.The DWTT shear area (SA) percentage of the clad steel produced using the TM process remained at 100% at -20 ℃.Therefore,if low-temperature toughness is not required in the pipe design,such as at -10 or -20 ℃,either process can be used.However,based on the results presented in Table 4,when a lower-temperature DWTT property is required,the TM process is a better choice.

Table 4 CVN impact test and DWTT results

3.2 Bonding requirements of 825 clad plate

3.2.1 Bonding rate requirement

In accordance with the design requirements,clad steel must meet the requirements of the ASTM A265 standard for Class 1 nickel and nickel-based-alloy clad plates.According to this standard,the bonding rate of the clad plate must not be less than 99%,wherein the maximum length of an unbonded single region must not exceed 25 mm.

The clad plates produced by the Q-T and TM processes were examined by ultrasonic testing with respect to the ASTM A578 standard.The results indicated that there was no difference between the plates produced by the two processes.No unbonded regions were detected.

3.2.2 Shear strength

The bonding rate is an important parameter that reflects whether the cladding and base materials have bonded.However,this parameter cannot characterize the bonding ability of the cladding and base materials.Thus,in addition to evaluating the bonding rate,shear strength was measured to determine the bonding abilities of the clad steels.According to the ASTM A265 standard,the minimum shear strength shall not be less than 140 MPa for nickel-alloy clad steels.

For safety reasons,however,higher shear strength of clad steel is desired due to its use in more severe environments.For some projects,the minimum shear strength required was not less than 250 MPa.

A comparison of the shear strength results of the Q-T and TM processes reveals that the average values ranged between 397-401 MPa,as shown in Table 5.These results indicate that both processes obtain excellent bonding strength between the cladding and base materials,and that there is no apparent difference in the strength data of the two processes.

Table 5 Shear strength of 825 + X65 produced using two different processesMPa

3.3 Microstructures at the bonding interface of the clad steels

As shown in Table 5,roll-bonded clad steels have high shear strength because the cladding and base materials are metallurgically bonded during the hot rolling or heat treatment.Fig.1(a) shows the electron backscatter diffraction(EBSD) microstruc-ture of the Q-T-treated clad steel.In the figure,the upper area shows the microstructure of the cladding material,i.e.,the 825 alloy,and the lower area shows the microstructure of the base material,i.e.,the carbon steel.As can be seen in the figure,around the bonding interface,there is an indistinct transition zone.In this transition zone,the microstructures are composed of incomplete austenite grains,with the remaining austenite components apparently miss-ing.However,at the boundaries indicated by the arrows in Fig.1(c),two continuous austenite grain boundaries are evident in both the cladding and base materials.This clearly shows that a whole grain occupies both layers.Thus,at high temperature,lattice reconstruction has taken place near the interface.The areas adjacent to the bonding inter-face gradually form an austenite grain with a regular lattice arrangement despite the inhomogeneous chemical composition.Fig.2 shows a schematic diagram of the recrystallization in the area around the bonding interface in the clad steel at high tem-perature.Two types of atomic diffusion occur around the bonding interface:the diffusion of interstitial atoms and the diffusion of substitutional atoms.If the clad plate remains at a high tem-perature for a sufficient period of time,the diffusion distance is long,i.e.,varying from tens of microns to even one hundred microns.However,the diffusion distance of the substitutional atoms is limited even at high temperatures,usually ranging from several microns to a little more than ten microns.In the recrystallized grains,the com-position is not homogeneous because most of the alloy-element atoms in clad steels are sub-stitutional,which requires a very long time to diffuse over a long distance.The resulting lattice reconstruction comprises disordered face-centered-cubic (FCC) austenite grains.As such,in the tran-sition zone,the atoms in the cladding and base materials bond.Fig.3 shows a schematic diagram of the evolution of an austenite grain across the bonding interface with changes in temperature.In the roll-bonded clad steel,interstitial atoms such as carbon and nitrogen diffuse much faster and sub-stitutional atoms migrate relatively slowly.Due to the distribution of composition in the transition zone,the region near the cladding layer has a greater alloy content,which can maintain the FCC structure from high to room temperatures.In contrast,the region near the base material has a lower alloy content (more closely resembling the composition of the base material),which can maintain the FCC structure at high temperatures but transforms into a body-centered-cubic (BCC) structure when the tempera-ture decreases.Therefore,it can be concluded that in roll-bonded clad steel,around the bonding interface,alloy atoms migrate to opposite sides to form a metallurgical transition zone.In the high-temperature range,this transition zone is composed of recrystallized austenite grains,but when the temperature is lower,these grains transform into two microstructures,whereby the upper component does not change and maintains the FCC structure,and the lower component transforms into a BCC structure,as shown in Fig.1(b) and Fig.3.

3.4 Microstructures and corrosion resistance

The microstructures of the clad steel produced by the Q-T and TM processes are compared in Fig.4.Fig.4(a) shows the microstructure of the clad steel treated by the Q-T process,in which the 825 nickel-based alloy contains recrystallized austenite grains,but near the bonding interface,the grain boundaries are more easily corroded when subjected to electrolytic corrosion.A 50-100 μm dark wide belt is evident along the interface.The scanning electron microscopy (SEM) micrograph in Fig.5 shows this belt more clearly.Near the interface,etching grooves are evident at the grain boundaries because carbon atoms have migrated from the carbon steel into the nickel-based alloy and carbides have formed along the austenite grain boundaries.In the steel produced by the TM process,no carbon atom diffusion zones were observed due to the limited time available for carbon diffusion.There-fore,for effective corrosion resistance,the required thickness of 825 treated by the Q-T process must include an additional 50-100 μm.

3.5 Intergranular corrosion and pitting corro-sion of clad steels

For the practical application of clad steels,both the mechanical properties and the corrosion resis-tance of the cladding material are key factors.Accord-ing to the ASTM standards and the customer’s require-ments,three testing methods are typically used to assess the corrosion resistance of the 825 alloy layer.These include the intergranular-corrosion-test standards ASTM 262 method C and ASTM G28 method A,and the pitting-corrosion-test standard ASTM G48 method A,which were used to evaluate and compare the clad steels produced by the Q-T and TM processes,as well as solid 825 plate,as shown in Table 6.From the table,it is evident that the cladding materials treated with the Q-T and TM processes both meet the strict requirements of the customer,and their corrosion rates are low and sufficient.The comparison of the corrosion results of the clad steels produced by the two processes and those of the solid 825 plates shows that they are very similar.

Table 6 Corrosion rates for cladding materials of 825 clad steels

3.6 High-temperature stress corrosion cracking test in simulated environment

Apart from the above intergranular and pitting corrosion results,high-temperature stress corrosion cracking (SCC) is a major concern of engineering users because it provides a much better indication of the performance of clad steels in the real service environment.Our tests were conducted according to ISO 7539-2 and NACE TM 0177 using the “four-point bending method” for the clad steels produced by the two processes.As shown in Table 7,the test conditions were selected to simulate an actual gas or oil field environment.After loading the actual yield stress of the cladding material,it was subjected to 720 h at 120 ℃ and a certain pressure in the simulated environment.The specimens were then observed using a 10× microscope,and no SCC was observed at the surface under tension of the steels produced by the two different processes.Fig.6 shows an example of the comparative results of the surfaces before and after the high-temperature test of the cladding-material steel produced by the TM process.In the figure,no cracks can be observed on the surface of the material.

Table 7 Simulated environment of stress corrosion cracking test

4 Conclusions

The mechanical properties and corrosion test results of this study reveal that clad steels manu-factured using the Q-T and TM processes can both meet the strict design requirements of projects involving the transport of gas or oil.

Due to the mutual diffusion of atoms between the cladding and base materials,a metallurgical transition zone forms,which results in high shear strength at the bonding interface.This transition zone is not obvious and is difficult to observe by conventional metallographic techniques.By using EBSD for the analyses of grain orientation,phase,and grain boundary reconstruction,it was found that at high temperatures,a transition zone formed and the atomic lattice in the transition zone was recon-structed to produce new austenite grains.When the temperature is lower,the alloy-element composition of the grains near the cladding material such as nickel and chromium is higher,so the FCC micro-structure remains even when temperature decreases to room temperature.However,in the region close to the base material,the composition of the alloy elements is closer to that of the base material of carbon steel.Thus,the austenite grains at high temperatures change from an FCC structure to a BCC structure at a lower temperature.

Our comparison of the Q-T and TM processes reveals that both can achieve the desired mechanical properties for alloys in carbon steels.The results obtained in this study show that the TM process may be a better choice for clad steel requiring low-temperature toughness.

With reference to solid 825 alloy,a comparison of the results obtained by the Q-T and TM processes reveals that the clad steels produced by both the Q-T and TM processes have excellent corrosion resistance.The major difference between the two pro-cesses is in their degree of carbon diffusion from the base material to the cladding material.The carbon diffusion distance was very limited in the TM-treated steel,whereas diffusion thickness of about 100 μm was observed in the Q-T-treated clad steel.

Acknowledgement

The work was partially funded by Shanghai Pujiang Program (No.16PJ1430200).The authors would like to appreciate Dr.Gong Yu at Shanghai Jiaotong University for his help in the EBSD characterizations.


登录APP查看全文