APP下载

低位错密度的XRD无损表征研究

2016-01-12苗瑞霞

科技创新导报 2015年5期
关键词:测量

苗瑞霞

摘 要:当半导体材料中位错密度大于107cm-2,难以用传统的腐蚀法进行测量时,可以利用高分辨X射线衍射(XRD)峰的半高宽估算材料中位错密度。该文利用该方法研究了位错密度小于107cm-2时是否适用的问题。结果表明,材料中位错密度较低(5.3×105cm-2)时,利用XRD测得的位错密度值与实际值存在3个数量级的偏差。分析认为,当晶体中位错密度较低时,参与衍射的晶面就越多,衍射峰就越窄,当位错加宽值与仪器精度接近时,就会产生较大偏差。因此在低密度位错时,利用XRD方法测量材料中位错密度时容易产生较大偏差。

关键词:XRD 4H-SiC 位错密度

中图分类号:O657.3 文献标识码:A 文章编号:1674-098X(2015)02(b)-0092-02

The Study of XRD Nondestructive Characterization at Low Dislocation Density

Miao Ruixia

(School of Electronic Engineering,Xian University of Posts and Telecommunications,Xian Shanxi,710121,China)

Abstract:It is difficult to measure by conventional etching method when the dislocation density of the semiconductor material is greater than the 107cm-2. Dislocation density can be estimate utilized in high resolution X-ray diffraction (XRD)peak half-width in this case. In this article, whether to apply using this method in less than 107cm-2 of the dislocation density is studied.The results show there has the three orders of magnitude of the deviation between measured values and actual values at. 5.3×105cm-2.Analysts believe that when the crystal dislocation density is low, the diffraction peak is more narrower. When the value of the dislocation widening approach to instrument accuracy, it will have a greater bias. Therefore, it will prone to large deviation when measured by XRD at dislocation density.

Key Words:XRD;4H-SiC;dislocation density

当半导体材料中位错密度大于107cm-2,很难用传统的腐蚀法进行位错密度的测量。目前常采用的方法是利用高分辨X射线衍射峰的半高宽估算材料中位错密度[1-5]。X射线衍射技术(XRD)是利用晶体形成的X射线衍射,对物质内部原子在空间分布状况进行分析的一种无损测试方法[6]。如果该方法在位错密度较小时仍适用,则该方法将成为首选的无损测量位错密度的方法。因此本文选用位错密度较低的4H-SiC材料对该问题展开了研究。

1 实验

4H-SiC单晶材料选用商用沿(0001)面偏切4°的N型材料。腐蚀设备为SX2-10-12箱式电炉,最高工作温度为1200°C。腐蚀剂为分析纯KOH,镍坩埚盛放腐蚀剂和样片,腐蚀样品在XSP-35TV型光学显微镜下进行观察。样品的X射线衍射测试在型号为D8 discover的仪器上进行,射线源为CuKα,射线波长λ为0.154nm。样品衍射面选(0004)面,扫描方式为3晶轴ω-2θ,仪器精度10arcsec。……

登录APP查看全文

猜你喜欢

测量
测量重量,测量长度……
测量的乐趣
二十四节气简易测量
日出日落的观察与测量
测量
测量水的多少……