氯丁胶在轨道车辆用粘接组件中的VOC释放性研究
2021-04-27卜繁强窦磊王庆文朱梅奇黄建赵吉君罗金黄德明王哲王咏祥
卜繁强 窦磊 王庆文 朱梅奇 黄建 赵吉君 罗金 黄德明 王哲 王咏祥



摘 要:为探究氯丁胶在轨道车辆用粘接组件中VOC的释放情况,文章利用袋子法对地板组件、防寒材组件及它们的组成材料分别进行VOC测试。研究表明,在粘接组件制样初期,氯丁胶对其VOC的影响明显高于其它组成材料;而随着放置时间的延长(至少21d),氯丁胶对地板组件中VOC的影响程度要大于相应防寒材组件中的。
关键词:氯丁胶;轨道车辆;粘接组件;VOC;袋子法
中图分类号:TQ331 文献标识码:A 文章编号:1001-5922(2021)07-0001-04
Study on the VOC Release of Neoprene in Bonding Components for Rail Vehicle
Bu Fanqiang1, Dou Lei1, Wang Qingwen1, Zhu Meiqi1, Huang Jian1, Zhao Jijun1, Luo Jin1, Huang Deming1, Wang Zhe1, Wang Yongxiang2
(1.CRRC Changchun Railway Vehicles Co., Ltd., Changchun 130062, China 2.Guangzhou Guangdian Metrology & Test Co., Ltd., Guangzhou 510656, China)
Abstract:In order to explore the VOC release of neoprene in the bonding components for rail vehicles, this paper uses the bag method to conduct VOC tests on floor components, cold-proof components and their constituent materials. The result shows that the effect of neoprene adhesive on VOC in bonding components is significantly higher than that of other materials at the initial stage of sample preparation, and with the extension of storage time (at least 21 days), the effect of it on VOC in floor component is greater than that of cold-proof component.
Key words:neoprene adhesive; rail vehicle; bonding component; VOC; bag method
0 前言
氯丁胶是一种具有初粘力大、粘接强度高的胶粘剂,也是第一种被大量生产的合成橡胶化合物,广泛用于轨道车辆、建材、制鞋等行业[1-4]。
2006年,国家铁道部颁布了TB/T 3139标准——《机车车辆内装材料及室内空气有害物质限量》 [5],该标准对机车车辆用胶粘剂中有害物质的限量及试验方法做了明确规定,但针对对象是胶粘剂液体,对固化后的胶粘剂并未作相关规定。2018年,钱秀敏等人[6]对照TB/T 3139标准,发现氯丁胶的总挥发性有机物(TVOC)含量在液态及固化(初期、7d和21d)时均远高于其他类型的胶粘剂。随后,张兰兰等人[7]利用加热失重和袋子法分别考察了各类胶粘剂在液态及固化1d时的TVOC含量,依旧发现其中氯丁胶含量最高,但其固化7d后TVOC含量便可明显降低88%~98%。
鉴于氯丁胶VOC含量普遍高于其它胶粘剂,且尚无粘接组件中氯丁胶的释放性研究。因此,本文分别对地板组件、防寒材组件以及它们的组成材料——地板、地板布、氯丁胶、防寒材分别进行随时间变化的VOC测试,以此探究氯丁胶在粘接组件中的VOC释放规律,为轨道车辆粘接组件环保性能提升提供理论依据。……