注氮气井井下设备腐蚀原因分析及相应对策
2017-10-14,,,,
, ,,,
(中国石油化工股份有限公司 西北油田分公司,乌鲁木齐 830011)
注氮气井井下设备腐蚀原因分析及相应对策
许艳艳,侯帆,丁保东,肖雯雯,刘冬梅
(中国石油化工股份有限公司西北油田分公司,乌鲁木齐830011)
塔河油田采用注氮工艺后井下设备发生了严重腐蚀。为确定造成腐蚀的主要原因,采用扫描电镜、X射线衍射仪和能谱仪等对井下腐蚀产物进行分析。结果表明:腐蚀产物中的元素以Fe和O为主,主要成分为Fe3O4,注氮工艺过程中夹带的氧气是造成腐蚀的主要因素;根据氧的腐蚀机理,提出了针对氧腐蚀的对策,如改变制氮方式控制氧含量,选择合适材料,对井下金属设备采用涂层、缓蚀剂、阳极保护等防腐蚀方法。
注氮气;腐蚀;氧;防护
Abstract: The down-hole device was corroded seriously after application of nitrogen injection technology in Tahe oil field. In order to determine the corrosion reasons, the down-hole corrosion products were analyzed by scanning electron microscopy (SEM), X-ray diffraction (XRD) and energy dispersive spectroscopy (EDS). The results show that the main elements of corrosion product were Fe and O, and the main composition was Fe3O4. Oxygen carried in nitrogen injection process was the main corrosion reason of the device. According to the corrosion mechanism of oxygen some countermeasures to control oxygen corrosion were proposed, such as changing the nitrogen production method to control the content oxygen, choosing proper materials, and corrosion protection of coating, inhibitor and anodic protection.
Keywords: nitrogen injection; corrosion; oxygen; protection
注氮工艺是提高采收率的主要方法之一。从2013年6月开始,塔河油田大规模采用了注氮工艺来提高产量,此工艺的实施使塔河油田的石油采收率获得了不断的提升。但在此工艺实施及后续生产过程中,井下油管、柱塞和抽油杆等设备出现不同程度的腐蚀结垢现象,这不仅影响油田正常生产,也增加了生产成本,腐蚀已成为该技术在现场应用中急需解决的问题。
1 塔河油田注氮气工艺概况
塔河油田注氮工艺主要应用膜制氮设备,注气压力23 MPa,井口温度30 ℃,氮气纯度约为95%,氧含量约为5%(质量分数)。图1为塔河油田制氮、注氮工艺流程图。