Preparation of Zr-Cu Coatings on Copper Substrate Using a Molten Salt Method
2023-10-07LIYushaZHANGYingchunLIUYanhongLIGuangbinDONGXiaoxun
LI Yusha ,ZHANG Yingchun* ,LIU Yanhong ,LI Guangbin ,DONG Xiaoxun
(1. School of Materials Science and Engineering, University of Science and Technology Beijing, Beijing 100083, China; 2. State Power Investment Corporation Science and Technology Research Institute, Beijing 100029, China)
Abstract: Dense zirconium coatings on copper substrates were obtained in an alumina crucible and a stainless steel crucible from FLiNaK-K2ZrF6 molten salt at 1 023 K.Due to the potential differences between copper and zirconium,zirconium can diffuse into the copper substrate to form zirconium alloys on the surface of copper substrates in the course of deposition.The coating deposited in a stainless steel crucible has a gray surface.The components of the coating are mainly CuZr2 alloy and Cu10Zr7 alloy,and,the outermost layer of the coating is a layer of amorphous pure zirconium.The coating deposited in an alumina crucible has a silvery white metallic luster.The components of the coating are mainly Cu-Zr-Al intermetallic compounds,AlCu2Zr,ZrAl,AlCu and CuZr.Furthermore,two types of zirconium coatings can greatly increase the hardness of the substrate.
Key words: coating;Zr-Cu;molten salt;intermetallic compounds
1 Introduction
Zirconium has a low cross-section of neutron capture.Under high temperatures or aggressive medium,zirconium has great corrosion resistance[1].Futhermore,zirconium has good physicochemical properties (excellent mechanical resistance,high pyrophoricity).Therefore,zirconium and Zr-based alloys are widely used in various industries such as nuclear field,aviation industry,electronics industry,medical industry,etc[2].Zirconium plays an extremely important role in the atomic energy industry[3].Most of zirconium metals are used as nuclear materials.In addition to being used as a nuclear material to prevent corrosion[4],zirconium alloys are also used as metallic glass because of their high strength and hardness[5].Therefore,more and more attention has been paid to the research and preparation of zirconium and zirconium alloys.In order to simplify the process,improve the efficiency and reduce the cost,many processes for obtaining zirconium or zirconium alloy coatings on the surface of non-zirconium metals have been studied[6-8].
Sitek[9]prepared Ni-Al-Zr coating by CVD,and found that the coating improved the corrosion resistance of Ni alloy against a Na2SO4solution.Linda Aissaniet al[10]investigated the structure and mechanical proprieties of Cr-Zr-N coatings,finding that Zr could contribute to the grain refinement of Cr-Zr-N films,and Zr increased the hardness and wearing properties of Cr-Zr-N films a lot.Stanislav Haviaret al[11]prepared Zr-Cu thin-film alloys by non-reactive magnetron co-sputtering.They found that Zr-Cu thinfilm alloys had high hardness and rigidity,good elastic strain and high yield strength by nanoindentation and microbending testing experiments.At present,zirconium is mainly prepared under high temperature conditions.It has been shown that molten salt process is an effective method for the preparation of zirconium and its alloys[12,13],and the coatings prepared by molten salt electrolysis process have good bonding properties with the substrates[14,15].The experimental equipment is relatively simple,and this method can reduce the preparation temperature[16,17].However,most of the researches studied the redox reactions of zirconium ion under the condition of applying power source.We offered a type of molten salt system which can complete the redox reactions without external power supply,and coatings of zirconium and zirconium alloy were deposited on the surface of copper substrates by relying only on the characteristics of the two materials themselves.It is a promising method to prepare zirconium and zirconium alloy because simple equipment is needed and coatings can be easily obtained on the surface of special-shaped samples.
2 Experimental
All the chemicals used in the experiments were anhydrous reagent grade.KF(purity: 99.95%),LiF(purity: 99.95%),NaF(purity: 99.95%) and K2ZrF6(purity: 99.95%) were dried in a furnace at 673 K for 24 h.The dried chemicals were well mixed into a eutectic composition (KF:LiF:NaF=46.5:11.5:42 mol%) and 6 wt% K2ZrF6was added into the mixture.Later,these chemicals were put into an alumina crucible and a stainless steel crucible(304 stainless steel).Then,these chemicals were melt in an electric resistance furnace.All the experiments were performed under argon atmosphere and the temperature of the molten salt was controlled with a K-type thermocouple.
A copper plate (purity: 99.95%,15 mm × 10 mm × 5 mm) and a zirconium plate (purity: 99.9%,15 mm × 10 mm × 1 mm) were prepared.Prior to the experiment,the surfaces of the copper plate and the zirconium plate were mechanically polished to obtain high quality surfaces and then they were cleaned with acetone and distilled water by ultrasonic cleaning.The processed copper substrate and pure zirconium plate were connected together with Pt wires and then placed into the crucibles.Then the temperature was slowly increased up to the experiment temperature(1 023 K)for 2 h.
The phase and crystal orientation identification of zirconium coating were examined by X-ray diffraction(XRD,Rigaku Indus-trial Co.,Ltd.,D/MAX-BB).The surface morphologies of the deposits were characterized by scanning electron microscopy (SEM,JSM6480LV).The cross section morphologies were observed by scanning electron microscopy (SEM,JSM 6480LV)with point analysis.Surface roughness of coatings was tested by laser scanning confocal microscope (LSCM,LEXT OLS4000 3D) for three times and an average value was selected.The microhardness of the zirconium coatings was measured according to Vickers microhardness test procedure using microhardness tester(MH-6) with a load of 200 g for 15 s and an average of 10 indentations was evaluated.
3 Results and discussion
3.1 Effect of crucibles on the crystal structure of the coatings
In order to analyze the structure of the coating,Fig.1 shows the appearance of the zirconium coatings prepared in different crucibles.It can be seen from Fig.1 that shiny coatings can be deposited in both crucibles,and the coatings uniformly and completely cover copper substrates.The coating deposited in the alumina crucible has a silvery white metallic luster,while the coating deposited in the stainless steel crucible has a gray surface.

Fig.1 Appearance of the zirconium coatings obtained in an alumina crucible and a stainless steel crucible
Fig.2 shows the SEM micrographs with EDS analysis of the coatings on copper substrates obtained in alumina crucible and stainless steel crucible.It can be seen from Fig.2 that the coatings on the surface of the two samples are uniformly dense and complete.From the EDS analysis,element Zr exists in both samples.Al exists in the coating obtained from the alumina crucible,which leads to the result that the surface is silvery white.But Al does not exist in the coating obtained from the stainless steel crucible.The coating mainly contains Zr with a small amount of Cu and C.
X-ray diffraction was used to analyze the composition of the coatings.Fig.3 shows the XRD pattern of zirconium coatings obtained in the alumina crucible and stainless steel crucible.It can be seen from the figure that when the alumina crucible is used,the components of the coating are mainly AlCu2Zr alloy,ZrAl alloy,AlCu alloy and CuZr alloy.When the stainless steel crucible is used,the components of the coating are mainly CuZr2alloy,Cu10Zr7alloy,and a small amount of pure zirconium.However,the content of pure zirconium in the coating is very small.

Fig.3 XRD patterns of coatings obtained in an alumina crucible and a stainless steel crucible
In order to analyze the distribution of elements in the coatings further,SEM with EDS was employed to characterize the surface and cross-section.Fig.4 shows surface and cross-sectional SEM morphology with map scanning of the coating obtained in the alumina crucible.Fig.4(a) shows the SEM image of the surface of the coating,and the EDS maps of Al,Zr and Cu,respectively,collected from this area.Fig.4(b) shows the SEM image of the fracture of the coating,and the EDS maps of Al,Zr and Cu,respectively,collected from this area.There are three elements that react with one another,which results in the reaction being complicated.According to the EDS analysis,three layers constitute the coating.The first layer which is close to the copper matrix is about 30 μm thick.There is a lot of Zr and Cu,and a trace of Al.The second layer is approximately 7 μm thick with little Al.The third layer,the outermost one,is approximately 3 μm thick.It is speculated that the third layer is a pure aluminum coating.But,it is too thin to be found in the XRD pattern.

Fig.4 The surface and cross-sectional SEM morphology with map scanning of the coating obtained in an alumina crucible: (a) surface;(b)cross-sectional
Fig.5 shows surface and cross-sectional SEM morphology with map scanning of the coating obtained in a stainless steel crucible.Fig.5(a) shows the SEM image of the surface of the coating,and the EDS maps of Zr and Cu,respectively,collected from this area.Fig.5(b) shows the SEM image of the fracture of the coating,and the EDS maps of Zr and Cu,respectively,collected from this area.The coating is approximately 40 μm thick and the coating roughly has three layers.The first layer,Cu10Zr7alloy,which is close to the copper matrix is about 10 μm thick.The second layer is a CuZr2alloy approximately 20 μm thick.The third layer,the outermost layer,is a pure zirconium coating approximately 10 μm thick.However,the XRD pattern shows less pure zirconium.It is speculated from the microstructure that the pure zirconium coating in the coating is amorphous.

Fig.5 The surface and cross-sectional SEM morphology with map scanning of the coating obtained in a stainless steel crucible: (a) surface;(b)cross-sectional
3.2 Effect of crucibles on the performance of coatings
Fig.6 shows the surface roughness of two samples.The surface roughness of the coating deposited in an alumina crucible is 0.036 μm,and in a stainless steel crucible 0.956 μm

Fig.6 Surface roughness of two samples: (a) in an alumina crucible;(b) in a stainless steel crucible
Fig.7 shows the vickers microhardness of three samples.The results indicate that the hardness of these two coatings is much higher than that of the copper substrate.Copper substrate has the lowest hardness of 98 HV.Zirconium coatings can greatly increase the hardness of the substrate.The coating prepared in the alumina crucible has the highest hardness(875 HV) because of its compactness and uniformity.The hardness of the coating prepared in the stainless steel crucible is 683 HV,which is much higher than that of the substrate.

Fig.7 Vickers microhardness of three samples
3.3 Deposition mechanism
The elements contained in the surface of the samples obtained from the two different crucibles are different,which can be seen from Fig.2 to Fig.5.The surface elements of the sample obtained from the stainless steel crucible are only Cu and Zr.The coating is a Cu-Zr alloy layer,and no element Al exists.The coating is mainly made up of Cu-Zr intermetallic compounds,CuZr2and Cu10Zr7,and the outer layer is a very thin layer of pure zirconium.Due to the different electric potentials between copper and zirconium,copper and zirconium connected with a Pt wire in a FLiNaK-K2ZrF6molten salt environment forming a primary cell.Fig.8 shows the schematic diagram of the deposition process of zirconium on the copper substrate.In this primary cell,zirconium served as the anode and copper served as the cathode.Therefore,pure zirconium sheet as anode would lose electrons and formed zirconium complex with F ions.Yeet al[18]found that ZrF73-was the only stable existence form of zirconium ion in FLiNaK-K2ZrF6molten salt through X-ray diffraction.The oxidation process on the surface of the pure zirconium sheet might have proceeded as:

Fig.8 Schematic diagram of the coating process obtained in stainless steel crucible
ZrF73-would form unstable low coordination number zirconium complex-ion in molten salt,which occurred as follows:
Copper substrate as cathode,the reduction process on the surface of the copper substrate proceeded as:
The metallic zirconium formed on the surface of copper substrates would diffuse with copper to form a diffusion coating.Because the sizes of the atomic radii of zirconium and copper are quite different,the original lattice structure would be destroyed during diffusion,and therefore an amorphous Cu-Zr alloy layer formed.When the diffusion stopped,a pure zirconium coating would directly form on the surface of the copper substrate.This pure Zr layer has the same potential as the anode,which could not meet a primary cell condition,that was,the deposition stopped.The Cu-Zr binary system has been widely studied as metallic glass materials due to its high strength and high hardness[5].The hardness of the Cu-Zr alloy coating is much higher than that of the substrate,which can be seen from Fig.7.
Element Al appeared on the surface of the sample obtained from the alumina crucible,indicating that element Al from the crucible has participated in the reaction.Liet al[19]studied the electrodeposition of aluminum on Cu substrates by cyclic voltammetry in molten LiCl-KCl-AlCl3,and obtained three different Al-Cu intermetallic compounds,Al4Cu9,AlCu,and Al2Cu.The presence of element Al was tested out on the surface of the sample obtained in the alumina crucible(Figs.2,3,4),indicating that during this deposition process,Al ions from the alumina crucible would be reduced to metal Al on the surface of the copper substrate due to the potential differences or current in the FLiNaK-K2ZrF6molten salt.Because the experiment involved the simultaneous reaction of Zr and Al in molten salt,the reaction processes were complicated,so further experiments and analysis were required.We can infer the deposition process from the experimental results.Fig.9 shows the schematic diagram of the deposition process of zirconium and aluminum on a copper substrate.Zr and Al are successively deposited on the surface of copper.Liet al[20]studied the diffusion process at the Al-Cu interface between 650 and 800 K,and the diffusion range of Cu and Al increased with the increase of temperature.In addition,Al has considerable solid solubility in the high-temperatureα-Zr[21].During this deposition,Cu-Zr-Al intermetallic compounds,AlCu2Zr,ZrAl,AlCu,and CuZr came into being as a result of the diffusion of Cu,Zr,and Al.When the condition of the primary cell disppeared in the experiment,the deposition stopped.The Cu-Zr-Al system also has high glass forming abilities[22,23].

Fig.9 Schematic diagram of the coating process obtained in alumina crucible
4 Conclusions
Both in an alumina crucible and a stainless steel crucible,dense coatings on copper substrates were obtained from a FLiNaK-K2ZrF6molten salt at 1 023 K.Because of the potential difference between copper and zirconium,primary cells can be formed in the FLiNaK-K2ZrF6molten salt,and Zr ions would be reduced on the surface of the copper substrates to form metallic zirconium.In the alumina crucible,element Al participated in the deposition process because of its high potential.At high temperatures,the metal elements would diffuse,resulting in Cu-Zr and Cu-Zr-Al diffusion coatings.The components of the coating are mainly CuZr2alloy and Cu10Zr7alloy.Furthermore,the outermost layer of the coating is a layer of amorphous pure zirconium.The coating deposited in the alumina crucible has three layers including AlCu2Zr alloy,ZrAl alloy and AlCu alloy.Both of the coatings have high density and uniformity,and can significantly improve the hardness of the samples.
Conflict of interest
All authors declare that there are no competing interests.
杂志排行
Journal of Wuhan University of Technology(Materials Science Edition)的其它文章
- Effect of Na+ and Sr2+ Substitution on the Formation of the Oxygen Vacancies in Y3Al2Ga3O12:Ce3+ Phosphor
- Stability of K-struvite in High Temperature and Acid-base Environment
- One-step Eco-friendly Fabrication of Antibacterial Polyester Via On-line Amination Reaction by Melt Coextrusion
- Photocatalytic Degradation of Rhodamine B by Recyclable AgBr/Polypyrrole(PPy) Nano-Catalysts
- Fabrication and Characterization of PMMA/MWCNTs Composite Materials
- Synthesis of Fluorene Derivatives Via TfOH-catalyzed Intramolecular Friedel-Crafts Alkylation Reactions