2022-11-02JovanMaksimovicJingwenHuSoonHockNgTomasKatkusGediminasSeniutinasTatianaPinedoRiveraMichaelStuiberYoshiakiNishijimaSajeevJohnandSauliusJuodkazis

Opto-Electronic Advances 2022年9期

Jovan Maksimovic, Jingwen Hu, Soon Hock Ng, Tomas Katkus,Gediminas Seniutinas, Tatiana Pinedo Rivera, Michael Stuiber,Yoshiaki Nishijima, Sajeev John* and Saulius Juodkazis ,6*

Keywords: silicon solar cells; laser ablation; light trapping; Lambertian limit

Introduction

Solar installations will soon provide 1 TW of power from~16TW we consume per year now with an annual uptake of solar increasing by ~ 35%1,2. Around the world,the most common type of photovoltaic installation is the venerable silicon solar cell, which has a typical efficiency of ~ 18%3. The efficiency of a hypothetical Si solar cell which perfectly absorbs all sunlight in the 300-1200 nm wavelength range and has no bulk or surface recombination losses is defined by the Shockley-Queisser limit of 32.3% at room temperature4. Real solar cells cannot absorb all such sunlight and even the purest silicon suffers from Auger recombination losses. The ray optics picture of light trapping suggests that solar absorption cannot exceed the so-called Lambertian limit. To go beyond the ray optics limit, a wave-interference-based light trapping solution needs to be engineered5(Fig. 1(a) and 1(b)). The Lambertian limit is given by the maximum of optical path enhancement in a weakly absorbing and optically thick mediumF=4n2, herenis the real part of the complex refractive index ~n=n+iκ. The Lambertian limit of absorbanceAL=αd/(αd+1/F), withα=4πκ/λbeing the absorption coefficient at the wavelengthλanddis the thickness of the cell.

It was recently shown that photonic crystals (PhC)made via surface texturing and targeting the 0.9-1.2 μm spectral range is the key to surpassing the light trapping Lambertian limit6. A thin 10-μm device layer of siliconon-insulator (SOI) was textured by inverted pyramid or tee-pee PhC structures of lattice constantΛ=2.5 μm or 1.2 μm, respectively (Fig. 1(c)). The demonstrated light trapping results propels the solar-to-electrical energy conversion to ~31%6. This performance was predicted theoretically and it is attainable with only ~ 10-15 μmthick Si7, which is very attractive for applications of lightweight flexible solar cells that can be coated on a variety of surfaces and have higher power conversion efficiency than present-day solar panels8. Flexible multi-junction solar cells are sought after in the automotive industry where high efficiency is required and there is a limitation of available surface area9.

Interdigitated back contacts (IBC) solar cells are currently the most efficient, breaking through the long-held 25% efficiency and performing above 26%, closing the gap to the Lambertian limit11,12. The final selection of an optimised surface texturing will be made upon full characterisation of the material's response11. Recently, it was shown that surface recombination velocity (SRV) in IBC Si solar cells can reach 10 cm/s after processing11. Surface nano-texturing by nanoscale needles - black-Si - can be utilised for anti-reflective function13. However, when black-Si was applied to Si solar cells, the best efficiency of only ~ 22% was achieved14. Also, a prohibitively high SRV value of ~ 100 cm/s was estimated on etched surfaces of black-Si15. It is not expected that the light-trapping methods based on ray-optics, when applied to conventional Si solar cell architecture, allows it to reach efficiencies beyond 28%5. The optimised IBC solar cells of 15 μm thickness with PhC light trapping should perform at ~30% efficiency even when SRV is as high as 100 cm/s5. The importance of good surface passivisation for Si solar cells16was demonstrated recently by record performing (26% efficient) both-side-contacted17and SiCbased highly transparent passivating contacts on 24% efficent cells18.

In this study, we compare two different methods to define and fabricate PhC light trapping on Si using etch mask patterning by: 1) direct laser writing by ablation and 2) stepper photo-lithography. For comparison, electron beam lithography (EBL) (as in ref.6) was also used.Process development and challenges are compared towards the goals of large area ~ 2×2 cm2fabrication of light trapping textures on Si, from the perspective of area up-scaling, throughput and technological bottlenecks.

Results

Laser ablation of etch mask

The simplest method to define a mask for plasma-based reactive ion etching (RIE) and/or wet etch of Si is directlaser ablation of sub-1 μm diameter holes in a film (Figure 2). Chromium, which is known for good adhesion to many different surfaces and is compatible with plasma and wet etch protocols of Si, was e-beam evaporated on Si and used for the mask. The refractive index of Si and Cr atλ=515 nm, the wavelength used for ablation, isn~Si=4.223+i0.061 and ~nCr=2.894+i3.323, respectively. The reflectance of Si and Cr (seeExperimental section) areRSi=38.1% andRCr=55.8%, respectively(note, for bulk samples). A film of chromiumd=30 nm thickness transmits onlyTCr=exp(-αCrd)=8.8% of pulse, whereαCr=4πκCr/λ. The absorbed component of the energyA=1-R-Tis utilised for ablation. This shows that energy is deposited almost exclusively into the Cr film, even if it is nano-thin (inset in Fig. 2(a)). For focusing with a numerical apertureNA=0.9 objective lens, the focal spot radius wasw0=0.61λ/NA=349 nm, the average fluence per pulseFp=Ep/(πw20)=0.26 J/cm2forEp=1 nJ and average pulse irradiance (intensity)Ip=Fp/tp=1.14 TW/cm2fortp=230 fs pulse duration. This coincides with the ablation threshold of Si~0.2J/cm219.

Fig. 2 | Cr etch mask defined by direct laser writing. (a) Calibration of the ablated hole diameter D2 ∝ ln(Ep) vs. the pulse energy Ep. The threshold 0.36 nJ (0.09 J/cm2, 0.41 TW/cm2) and 5.15 nJ (1.35 J/cm2, 5.85 TW/cm2) are the intersections of dashed-lines with x-axis. The solidline is expected evolution of D2 defined by the beam waist r = 0.61λ/NA. Top-inset shows light field E simulations for the NA = 0.9 focusing used with a Cr film on Si, for λ = 515 nm; the finite difference time domain (FDTD, Lumerical) was used. (b) SEM image of the ablated 30 nm Cr film;Ep = 1.7 nJ. The inset shows a closeup view of the ablated holes in the Cr film; the thumbnail image of the Airy pattern of the focal spot is scale matched. (c) SEM image of sample after 10 min plasma etch. The contrast change reveals the width W of the plasma etched Si (SF6:CHF3:O2 at 5:1:1 flow rate ratio). The inset shows photo of 2 × 2 cm2 area of ablated Cr mask on Si (before etch).

A detailed summary of the widthWevolution during etch time for different diameter holes in Cr-mask ablated by correspondingly different single laser pulses of energyEpare presented in Fig. S2. We took advantage of the semi-transparent nature of the 30 nm Cr mask in the SEM to explore structure changes during etching. For pulse energies ~ 1 nJ, Si:Cr alloying took place instead of ablation (see Supplementary information for details).This was evidenced during etching when those regions acted as a mask rather than a hole. When pulse energies exceeded ~8 nJ, less regular ablation craters were observed, which showed crack development in Cr mask after long>10 min etching times. Under etch of Si via ablated hole in the Cr mask was slow and followed slopeW ∝Eγpwithγ<1/2 (Fig. S2). Silicon under etch below the Cr-mask showed an anisotropy guided by the crystallinity of the ( 100) Si plane, which is most pronounced in the case of wet etching in KOH when inverted pyramids are formed. This anisotropy was responsible for the formation of under etch which was slowest in the diagonal direction of tee-pees and caused formation of protruding corners (marked as cones in Fig. S2(b)). Interestingly, the metal masks are known to facilitate under etch even for amorphous substrates21and could be used for more intricate control of the pattern. Once neighbouring tee-pee pits separated byΛ=3 μm approached each other, the narrow ridges were formed (Fig. S2(b)). For longer etching, PhC patterns became deeper, however,the depthHand widthWof individual tee-pees did not change.This conditionwasfurtherexploited for thenarrowestridgesR′. Tensofminuteswas enoughtoetch PhC structures. We used a slightly thicker Cr film of 50 nm for longer plasma etch to ensure complete under etch and the narrowest ridges in earlier studies of phenomena presented (Fig. 3). The under etch is illustrated by a pyramidal tip which formed in the place of missing ablation hole in the mask (as shown in Fig. 2(b)). Patterns of tee-pee PhC etched in the case of under etch showed similarity to those obtained by anisotropic wet etchning in KOH. Wet etching through ablated holes ofD ≈0.5 μm was taking ~ 14 hours in 30% KOH at 4 5 °C. Plasma etching took only tens of minutes for similar PhC patterns.

Fig. 3 | SEM images of a hard mask for RIE made in 50-nm-thick Cr film by laser ablation with 515 nm wavelength, 230 fs single laser pulses. Etched pattern after Cr mask removal. The inset shows an under-etch in the region where one ablation opening in the mask was absent.Conditions: NA = 0.9 lens was used, write speed 10 cm/s, pulse energy 5 nJ, laser repetition rate 200 kHz.

A dielectric alumina Al2O3film of 20-30 nm, which serves as a part of an antireflection and passivation coating of IBC cells11, can be used for fabrication of PhC patterns on Si using the same laser ablation method demonstrated for Cr at slightly larger laser pulse energy(Fig. S3). A simpler solvent-based ultrasonic bath removal of the alumina mask after plasma etching is another advantage of this processing, which avoids metal-ion wet chemistry.

Finally, to show capability to process thin Si wafers of 10μm thickness which is the target for a PhC enhanced light trapping, the same laser processing of Cr mask and plasma etching was carried out (Fig. 4). Si 2 ×2 cm2samples were laser cut from the micro-thin wafer using the same fs-laser with focusing objective withNA=0.14(Fig. 4(a)). For handling, the thin Si film was attached to a 4-inch sapphire wafer using resist, AZ1518. The resist is spin coated to be 1.5 μm on the sapphire wafer which acts as an initial carrier substrate, with the resist acting as an intermediary layer between the thin Si and the sapphire. This can be subsequently handled by laser cutting the Si to a desired size (Fig. 4(a)) and later put into a solution with developer for transfer to a new carrier substrate in the same way as previously mentioned for PhC patterning. It is important to have a very uniform resist film, to keep the attached Si as flat as possible making fabrication conditions ideal. Strong under etch below the Cr mask defined smaller ridgesR′for smaller periodΛfor the PhC as compared with largerΛ(Fig. 4(b)). The under etch is manifested by different heights of the PhC patterns with different periodsΛ=3 μm and 1.5 μm which were laser ablated on Cr mask side-by-side.

Stepper patterning of etch mask

Steppers reduce and project patterns from a reticle onto a silicon wafer. A 5×reduction means that the reticle does not require high-resolution electron beam lithography for it's fabrication, even when the resultant pattern is sub-micrometer. The smallest size on the reticle was a 2-μm-diameter disc, which will produce a 400 nm pillar (ideal conditions) on the etch mask for the Si solar cell. We used Sumiresist PFI-38 photoresist spin coated over 30-50 nm thickness Cr coatings (e-beam evaporated) for mask fabrication. After fabrication (a wet etch)the diameters of the holes in Cr-mask ranged from 180 nm to 245 nm with uncertainty ~ 10 nm (Fig. 5). Patterns with smaller periodΛexperienced a smaller UV exposure dose through the mask, which resulted in less proximity exposure (Fig. 5(b)). Top inset shows the actual shape of chromium-coated polymer pillars. Consequently, less exposure through optically blocked areas in reticle occurred and resulted in the larger diameter pillars obtained after development. This difference is illustrated by measuring the diameter of the opening in the chromium-mask after the lift-off (hole is formed in the location of the resist pillar). The hole diameters and their dependence on the period of the PhC pattern are shown in the inset of Fig. 5(b). To achieve ~ 200 nm holes in a 50 nm chromium film is evidence of the high resolution fabrication achieved for patterns defined by stepper photo-lithography. The critical fabrication step was lift-off. Pillars taller than 5 00 nm were required for successful lift-off of the 30-50 nm chromium film (see insets in Fig. 5(b)). Lift-off was not successful for smaller pillars, resulting in missing nano-holes in the mask.

Fig. 4 | (a) 10-μm-thick Si wafer cut by Ep ≈ 0.8 μJ energy fs-laser pulses (1030 nm/230 fs/200 kHz) using NA = 0.14 objective lens at 1 cm/s scan speed (5 passes with focus on the surface). SEM image of the 10-μm-thick Si wafer after cutting and patterning. Optical image of the 100-mm-diameter Si wafer on a plastic film. (b) PhC surface etched through holes ablated by fs-laser to define the Cr etch mask; NA = 0.9 lens was used, write speed 10 cm/s, pulse energy 12 nJ, laser repetition rate 200 kHz. Note the step height between regions with different period Λ. This step change is due to the under etch which is also responsible for formation of the upward-pyramid shown in inset of Fig. 3(b).

Fig. 5 | (a) Photo of the dot patterns (resist on Si) after exposure, development and dicing. Insets: (bottom) image of the entire 6-inch Si wafer after exposure and development; (top) the stepper reticle used for the i-line (365 nm Hg) 5× reduction (positive resist: the exposed regions are removed). (b) SEM images of 50-nm Cr film e-beam evaporated on 700-nm-thick resist patterns before and after lift-off; exposure was made by projection lithography on Si. Circular marker shows d = 200 nm for comparison with developed holes. Bottom-insets shows slanted-view images of the patterns after lift-off. Top-right inset shows the hole openings D for the four segments of PhC patterns with different periods shown in (a).

Electron beam definition of etch mask

We used conventional Si-wafers since IBC cell geometry is not compatible with SOI layer stacks. Cr masks were patterned by EBL to define PhC pattern with subsequent wet KOH etching. Figure 6(a) shows final PhC with μm made on four regions. Chromium coating helped with charge removal and surface positioning (height) for EBL writing. Small ridgesR′= 40-80 nm between neighboring inverted pyramids were obtained for longer KOH etch, however, more defects were observed when adjacent pyramids merged due to localised under etch. The number of defects was between 0.1 to 0.9%, calculated per 1 03pyramids. Figure 6(b) shows optical near-IR to IR performance of a 5 00 μm thick Si wafer patterned with the light trapping PhCs. The portions of reflected and transmitted parts of light intensity are from direct measurement and the absorbed portion is calculated from energy conservationA=1-R-T. The PhC surface pattern caused a spectrally wide anti-reflection effect which contributed to the larger portion of absorbed energy.This is evident from the difference between a patterned vs blank wafer spectra. Such surface can find applications in optical sensors (strong absorption) and emitters in the IR spectral range22,23.

Figure 7 shows a summary of the spectral characterisation made of different samples in this study; reflectance from the stepper lithography prepared samples was reported in ref.24, where the highest aspect ratio patternsH/W ≈1showed the lowest reflectivity. Similar tendency was observed for the PhCs defined by the laser ablated and EBL defined masks (Fig. 7). Figure 7(a, b) panels show high repeatability ofRspectra measured from four different regions of PhCs defined via EBL (a perfectly overlapping spectra). Reflectivity below≈8% was obtainable for PhC defined by different methods as long as ridges were narrow and width of the tee-peeW→Λ.The least reflective surface was observed from PhC structures which had corner regions between neighbouring tee-pee pits reaching the level of original Si surface (below Cr mask; see Fig. S2(b)). They were among the deepest structures withh ≈2.5 μm (marked as cones in Fig.7(c)). The tendency of reduction of reflectanceRwith under etch, which also caused narrowest ridgesR′→0,is apparent (see SEM thumbnail images in Fig. 7(c)).When inverted pyramids were etched by wet KOH or dry plasma processing (Fig. 7(c-2), Fig. 7(c-6)),R >10%was observed due significant contribution of original Si surface (at ridges) to reflectivity. Application of an antireflective coating for the final solar cell will provide further reduction of reflectanceR <1% and is required passivisation for the reduction of the surface recombination rate. The most promising samples for the practical solar cells will be those with strongly under etched tee-pees due to their low reflectivity and maximum of the removed material which was at a Si-mask interface. The used plasma etch of Si was carried out at low-bias and low-power which makes only shallow ~10 nm surface modification, which is fully recoverable to almost pristine surface quality by different post-processing steps of annealing, H2, O2treatments, or their combination,dependent on the used plasma chemistry25,26.

Fig. 6 | (a) Photo of large 2 × 2 cm2 light trapping PhC patterns KOH etched through a chromium-mask defined by EBL; period Λ = 3.1 μm. SEM images of the final PhC pattern on 500-μm-thick n-type Si(100) wafer. (b) Color-coded presentation of portions of the absorbed A, reflected, R(measured) and transmitted T = (1 - R)10-OD (measured) light at different wavelengths from 1.67 to 25 μm (or 6000-400 cm-1 in wavenumbers~ν= 1/λ).

Fig. 7 | Spectral characterisation of PhC light trapping. (a) Reflectance R measured with an integrating sphere for a Si wafer, PhC on SoI(see Fig. 1(c)), and PhC defined by EBL. Note all four segments (top inset in (b)) showed the same (overlapping) spectral profile. Top inset shows (n + iκ) components27. Interference fringes of SoI sample are defined by Si thickness t = λ1λ2/[2n(λ2- λ1)] ≈ 11 μm (near-IR; n = 3.46). (b)Portions of reflected R (measured), transmitted T (measured) and absorbed A = 1 - R - T portions. Inset shows a photo of the 4-inch wafer with 4 EBL defined PhCs. (c) Reflectance of different PhC patterns prepared by laser writing and EBL which were either plasma and wet etched (note lg-axis for R). The light spot size on the sample was ~ 2-3 mm in diameter in order to reproduce the same conditions on samples with different areas (see the inset in (a) showing sample illuminated inside the measurement chamber).

With optical theR(λ) andT(λ) measured experimentally, the absorbed partA(λ)=1-R(λ)-T(λ) can be accessed. Then, the maximum achievable photo current density (MAPD) of the solar cell under AM1.5 (Fig. 1(a))illumination of intensityIAM1.5(λ) can be calculated6:

where the constants are: e is the electron charge,his the Plank constant,cis the speed of light. It is assumed that each absorbed photon creates a single electron-hole pair.Consequently, the short-circuit currentJSC=JMAPDfor an ideal solar cell without losses due to surface and bulk recombination. How to achieve the latest conditions is an another wide field of research, which is already well matured and achieved world record efficiency in Si solar cell performance. Addition of PhC light trapping is a natural next step to improve light-to-electrical power conversion.

Discussion

Laser patterning of a Cr or Al2O3mask has the fundamental advantage of not using vacuum chambers for the lithography step for pattern definition and can be upscaled for large area fabrication. By combining high stage scanning speeds (10 cm/s and faster) with high repetition rates (200-600 kHz), it was possible to efficiently pattern 1×1 cm2surface areas within a reasonable~2 hours time. Beam travel speeds of meters per second are in reach using galvano and polygon scanners. Synchronising the stage movement with laser repetition rate results in good alignment of the ablated sites between neighbouring lines, at expense of a slightly longer writing time. Different Cr thicknesses necessitate different pulse energies to open holes in the mask, but 20-60 nm Cr film can be ablated with good control of hole diameter with sub-20 nJ single pulses. Such pulse energies are now available from fs-laser oscillators and regenerative amplifiers are not required. Due to the almost 2×sized holes ablated by laser writing as compared with stepper photo-lithography defined mask, approximately 2×faster plasmaetching wasobserved.Indeed,4 minwasallthat wasneededto achieveoptimalridgeconditionsR′→0 nm with the same optimised etching recipe for mask made by laser ablation.

In areas where there were missing holes at the laser ablation sites (missed pulse, slight change in spatial laser mode, etc.), an interesting pattern developed after under etch (Fig. 3(b)). During the initial etch, the expected inverted pyramid pattern formed under the mask. When etching of the PhC pattern continued through to under etch, an upward pyramid was formed at the location where intended hole was not ablated. These unexpected defects are therefore favourable for the creation of deeper PhC patterns since the crystal orientation of the Si precludes aspect ratios much greater than 1. The results suggest that by creating a checkerboard hole pattern instead of a regular array, each inverted pyramid will be surrounded by four regular pyramids. The resultant PhC will have double the spatial frequency. This type of defect-mode can be intentionally designed to fabricate deeper PhC patterns and will be explored further.

Future studies will focus on changing the ratio of SF6to CHF3to affect the anisotropy (difference in etch rate between inx-yandz) during the dry etching28. Tilted angle etching of Si was tested29, however, there was a strong difference in depth of the etched pattern at different distances from the electrode. Hence, using this method to control the shape of etched pits is less promising for PhC textured surfaces on solar cells even if predicts a close to Lambertian light trapping30.

With RIE, varying the bias power greatly influences the etch anisotropy, which is important since the underetch and aspect ratioH/Wcan be controlled. Anisotropic etching at a larger bias creates deeper patterns, while isotoropic sideways etching is enhanced by a larger inductively coupled plasma (ICP) power. It was found that the bias voltage had little effect on the aspect ratio of inverted pyramids. TheH/W ≈1 was observed (0.71 expected from Si lattice) and anisotropy of the Si etching was the defining property regardless bias used.

Conclusions and outlook

Two different fabrication methods for large-area(2 ×2 cm2) PhC patterns on Si for light trapping are demonstrated: 1) direct laser write and 2) stepper photolithography. They can scale up for light trapping solutions on order of magnitude larger surfaces and were compared with EBL, which recently showed close to the Lambertian limit performance over the visible spectral range and exceed it over 950 -1200 nm wavelengths when an antireflection coating was applied on SOI samples6. In this study, large 2 ×2 cm2areas are demonstrated using a Cr etch mask on a Si wafer, rather than on SOI samples, making them more promising for integration with the most efficient IBC geometry solar cells.

Holes of 350-400 nm were opened in a Cr or Al2O3mask by single laser pulse irradiation, with writing speeds of 10 cm/s. Smaller holes with 180-245 nm diameter were fabricated in the Cr mask by the second method, stepper projection photo-lithography and liftoff. The plasma etching rate of Si vs hole diameter,W, in Cr mask was sub-linear. Larger holes are vital for faster KOH etching, which is considerably longer ~10 h as compared with ~ 10 min for similar PhC patterns with RIE. Pulses of only 2-5 nJ (515 nm/230 fs) on the sample focused by aNA-0.9 dry objective lenses are required for laser printing of ~400 nm diameter nano-holes in the Cr-mask; approximately double the pulse energy was required for opening holes in the Al2O3mask.

Due to strong under etch, the surface of Si where damage occurred during hole ablation is removed by plasma etch. A subsequent KOH or TMAH31etch step for Si surfaces can be added for the lowest SRV and best quality at the very end of PhC fabrication. Use of dielectric Al2O3mask is expected to help further reduction of SRV and simplify surface texturing steps.

Future improvement of large area fs-laser pattering could employ Bessel-like beams to increase tolerance to surface tracking32and adopt stitch-free laser writing33.The main advantage of direct laser writing is due to it’s vacuum-free mode of operation in mask definition. Over the last 20 years, the trend for the average power of ultrashort pulsed lasers has been to double every two years,analogous to Moore’s law scaling34as reported by Amplitude Ltd. lasers35, i.e. the number of photons packed in time (power) scales like the transistors per area/volume on a chip. Flexibility of material processing by burst mode ablation36,37has fueled larger-area>1 m2industrial applications such as hydrophobic and anti-ice surface treatments or injection mold texturing38,39. Fast polygon scanners with beam travel speeds up to hundreds of meters per second have been implemented to disperse ~kW radiation power. These trends are promising for solar cell texturing on increasingly larger areas by direct laser writing demonstrated in this study.

Experimental section

The energy balance of the absorbed, reflected, and transmitted parts of light energyA+R+T=1 was calculated from the refractive index ~nof solar cell material (Si in this study27) at the normal incidence asR=[(n-1)2+κ2]/[(n+1)2+κ2] andA=1-R=4n/[(n+1)2+κ2]. These expressions are valid for light incidence from airnair=1. The Beer-Lambert law defines the transmitted partT=e-αdin a single pass through thicknessd;αd ≡ln(10)OD, where the optical density (absorbanceA) is calculated from the transmittance asOD=-lgT. From the known spectrum of Silicon permittivityε(λ)=n~(λ)2, the efficiency of light harvesting by different Si solar cell thickness was estimated and compared with the corresponding Lambertian limit.Three different methods to define a light trapping PhC pattern on Si solar cell surface are described next.

Femtosecond laser writing

Direct fs-laser writing by ablation of Cr-on-Si mask was carried out with a solid state Yb:KGW laser (Pharos,Light Conversion, Ltd. Vilnius, Lithuania) at theλ=515 nm wavelength withtp=230 fs pulses at repetition ratef=200kHz. High precision mechanical stages with write speed up to 25 cm/s (Aerotech, GmbH. Pittsburgh,USA) were used for the lateral in-plane (xy) translation of the sample during laser write. Axial (z) positioning of the focal spot onto Si surface was made by a high-precision stage mount of the objective lens. A software-hardware integration solution of the entire fs-fabrication unit was made by Altechna Ltd. Ablation was carried out with focusing using objective lens with numerical apertureNA=0.9 (Mitutoyo) at a low pulse energyEp=2-15 nJ (on the sample) with pulse-to-pulse separation for specified period of PhC fromΛ=1 μm to 3.1 μm. The laser beam profile was measured utilising a Ophir Spiricon SP928 beam profiling camera.

Laser fabrication was carried out in air (cleanroom,class 1000). Crystalline c-Si (n-type; Phosphorus-doped)〈100〉and intrinsic samples (University wafer) The conductivity and its type of Si was determined by the van der Pauw method with an Ecopia HMS-3000. There was no difference observed for the tested low conductivity intrinsic n- and p-type Si in terms of formation of the laser ablation patterns and PhC plasma etching.

All samples were cleaned in acetone and isopropyl alcohol (IPA) prior and post etching to minimise surface contamination. A Cr thin film deposition on Si was made by an electron beam evaporation (Kurt J. Lesker AXXIS system) A reactive ion etching (RIE) was carrier out with RIE-101iPH (Samco) equipped with a load-lock system. Structural and optical characterisation of laser ablated regions and PhC structures were carried out by the SEM operation mode of EBL writer (Raith EBL 150TWO).

Stepper photo-lithography

An i-line (365 nm) stepper NIKON NSR-2205i12D at Nano-Processing Facility (NPF) AIST, Tsukuba, Japan was used for this study. A reticle mask (inset in Fig. 5(a))consisting of four square regions with different PhC period,Λ, between a square array of 2 μm diameter disks (a light block for positive resist) were designed over the uniform exposure field of 10×10 cm2. The pattern was projected on a 6-inch Si wafer using a 5× demagnification with repeated exposure using the i-line stepper.Each quarter segment was a ~1×1 cm2area after the exposure (Fig. 5(b)). This pattern formed the mask for etching the photonic crystals (PhC).

An adhesion promoter for photoresist Hexamethyldisilazane (HMDS) was applied on Si wafers by dip coating after which 700 nm of positive resist (PFI-38) was spin coated onto the 6-inch Si substrate. After pre-baking at 90° for one minute, an exposure of 25 regions over 6-inch Si wafer was carried automatically (step & repeat;inset in Fig. 5(b)). Different exposure time (sub-1 s) was programmed for each step to optimise the exposure dose(~ 200 mJ/cm2is required to expose the resist). Post-exposure bake at 110° for 60 s was implemented. Development of resist after exposure was carried out for 10 s in NMD-3 2.38% tetramethylammonium hydroxide(TMAH). The unexposed regions were retained on Si after development and the wafer was diced into2×2 cm2chips after development (Fig. 5(a)). Then, e-beam evaporation of 50 nm of Cr was carried out as described in the previous section. By sonication for 30 min in acetone at room temperature, lift-off over the entire chip area was achieved. The mask was designed to obtain 400-nm-diameter pillars after development (corresponding to 2-μm disks on the reticle). The designed value was approximately twice the achievable resolution of 200 nm for the stepper used.

Electron beam lithography

A Vistec EBPG5000plusES EBL writer was used for definition of the KOH wet-etch masks. Two approaches were used, the first produced a Si3N4mask, the second produced a Cr mask. The first approach used a combination of LPCVD of Si3N4, E-Beam Lithography (EBL) and Deep Reactive Ion Etching (DRIE) to transfer the patterns into the Si3N4. The fabrication started from growing 250 nm Si3N4on both sides of an SOI substrate with 10 μm-thick device layer (inset of Fig. 1(c)). Both, plasma enhanced and low pressure chemical vapour deposition(PECVD & LPCVD) were tested to form the mask layer.The LPCVD was chosen since it provided more homogeneous, low stress, and porous-free films. A positive ZEP520 EBL resist was used for patterning. The array of patterned squares was oriented to align with the Si wafer flat. After development, the EBL exposure left a grid pattern of unexposed ZEP520 outlining the exposed Si3N4square areas. The width of the outline made of unexposed ZEP520 resist was optimised in the design step considering the under-etch of Si below the mask. The resulting ZEP520 grid was used as a mask for DRIE of the Si3N4layer below. After DRIE and stripping the resist, the final mask consisted in a Si3N4grid pattern outlining exposed square areas of Si. Particular care was taken to fully open the patterned areas into the Si3N4in order to expose the Si underneath while preventing excessive etching of the Si substrate. After KOH etching,the Si3N4mask was removed with HF. The final device was cleaned with Piranha solution. Photo-lithography was used to define back-side locations for eventual Si etching using AZ-family resist followed by RIE etch of Si3N4and stripping of the residual resist mask.

In the second approach, a Cr mask was made by EBL,Cr e-beam evaporation and lift-off. This approach was carried out on 4-inch Si〈100〉n-type Phosphorousdoped wafers with a resistivity of 1-10 Ω cm (111.75 Ω/□sheet resistance measured by 4-probe method (Jandel RM3000)). The outline of the squares was defined by exposing a 300 nm-thick layer of PMMA resist, leaving after resist development an array of regularly spaced PMMA squares. The patterned grid was oriented to align with the wafer flat. The spaces between the PMMA square patterns were filled with Cr by e-beam evaporation. The excess Cr and unexposed resist was removed during lift-off process with acetone. The result was a grid mask of Cr outlining the exposed Si square areas. After KOH etching, the Cr mask was removed using Cr etchant solution. The final device was cleaned with Piranha solution.

Etching

For potassium hydroxide (KOH) etch, a solution was prepared using 2 litres of 30% KOH which was then saturated with isopropyl alcohol (IPA) (2 cm surface layer).Etching was carried out at 4 0°C. The etch time was evaluated using an online calculator40for the known pattern to be etched. Level of p-doping strongly affected the etch time. The depth of the inverted pyramids was dependent on the periodΛof the light trapping texture. For the base-angle of pyramidβ=54.7°, the depthH=(Λ/2)×tanβand the side-length at the central cross section of a pyramids=(Λ/2)/cosβ. For the usedΛ=0.8,1.3,2.5,3,1μm, the corresponding depth (for ridge-less inverted pyramids pattern) ish=0.57,0.92,1.77,2.19μm (the aspect ratiosH/Λ=0.71). After etching the light trapping pyramidal texture, the front-side was protected by a Protek coating41before a back-side etch step through the SOI substrate. For thicker silicon (~ 300 μm), the KOH solution was heated between 60-70 °C to reduce etch time.Characterisation of fabricated structures was carried out using scanning electron microscopy (SEM), Fourier transform IR micro-spectroscopy (VERTEX 70 Burker),and UV/Vis/NIR spectrometer (PerkinElmer Lambda 1050).

Plasma etching of tee-pee patterns was carried out with SF650 sccm, CHF310 sccm, O210 sccm for 5 to 30 minutes (etch time dictated different structures); the RF ICP was 180 W, bias 0 W, He pressure 2.70 kPa at a process pressure of 2.5 Pa. Etching of black-Si was made by process: SF677 sccm, O2100 sccm for 5 min at RF ICP 300 W, bias 5 W, He pressure 2.70 kPa and process pressure of 2 Pa.