Adsorption behavior and mechanism of copper ions in the sulfidization flotation of malachite
2022-09-07HnWngShumingWenGungHnYongxinHeQichengFeng
Hn Wng,Shuming Wen,Gung Hn,Yongxin He,Qicheng Feng,*
a State Key Laboratory of Complex Nonferrous Metal Resources Clean Utilization,Faculty of Land Resource Engineering,Kunming University of Science and Technology,Kunming 650093,China
b State Key Laboratory of Mineral Processing,Beijing 100160,China
c Yunnan Key Laboratory of Green Separation and Enrichment of Strategic Mineral Resources,Kunming University of Science and Technology,Kunming 650093,China
d Inter Mongolia Xingye Mining Company Limited,Chifeng 024028,China
Keywords:Malachite Sulfidization flotation Copper ions Adsorption
ABSTRACT Malachite is one of the main minerals used for the industrial enrichment and recovery of copper oxide resources,and copper ions are unavoidable metal ions in the flotation pulp.The microflotation,contact angle,and adsorption experiments indicated that pretreatment with an appropriate concentration of copper ions could improve the malachite recovery,and the addition of excess copper ions reduced the hydrophobicity of the malachite surface.The results of zeta potential tests indicated that sodium sulfide and butyl xanthate were also adsorbed on the surface of malachite pretreated with copper ions.X-ray photoelectron spectroscopy (XPS) results indicated that —Cu—O and —Cu—OH bonds were formed on the surface of the samples.After pretreatment with an appropriate concentration of copper ions,the number of —OH groups on the mineral surface decreased,whereas the number of Cu—S groups on the mineral surface increased,which was conducive to the sulfidization of malachite.After adding a high concentration of copper ions,the—OH groups on the mineral surface increased,whereas the number of Cu—S groups decreased,which had an adverse effect on the sulfidization flotation of malachite.Time-of-flight secondary ion mass spectrometry showed that pretreatment with copper ions resulted in a thicker sulfidization layer on the mineral surface.
1.Introduction
In nature,the common copper oxide minerals are malachite,chrysocolla,azurite,and cuprite[1–3].The metallogenic conditions of oxidised copper deposits mainly evolved from the upper layer of copper sulfide deposited through long-term oxidation [4].Most copper oxide minerals are associated with other metal minerals[5],which present some difficulties in industrial beneficiation processes.Therefore,the enrichment of oxidised copper ore has always been an important research topic for beneficiation.With the improvement and development of mineral processing technology,the utilisation of oxide mineral resources has gradually improved.At present,flotation and leaching are typically used to enrich copper oxide minerals [6,7].
The flotation of oxidised copper ore can be divided into direct flotation and sulfidization flotation [8,9].Among current flotation processes,sulfidization flotation is the most widely used method for flotation recovery of copper oxide ores[10].Many factors influence the process of mineral sulfidization flotation,such as the amount of sulfidizing agent,pH,and temperature in the sulfidization process [11–13].Research has shown that if insufficient Na2S is used in the flotation process,copper oxide will not be completely sulfidized and thus cannot be effectively enriched.Conversely,if too much sulfidizing agent is added,the mineral will be restrained by the excessive amount of sulfide in solution,which will lead to a low recovery of copper oxide [11].Temperature has a significant effect on sulfidization,with higher temperatures providing a better sulfidization effect on the mineral [12].
The addition of an appropriate amount of regulator can improve the flotation recovery of minerals [11,14,15].Studies have shown that adding ammonium sulfate,ethylenediamine,and some metal ions can effectively the sulfidization of copper oxide minerals[1,9,11,15,16].The adsorption of S species on the malachite surface increases and leads to an increase in Cu—S species after modification by ammonia.In addition,ammonium sulfate on the malachite surface leads to lattice defects and provides favourable conditions for the adsorption of Cu(NH3)2+and S2-[11,15].Therefore,the sulfidization flotation recovery of malachite is effectively improved.The Cu (II) species on the mineral surface are reduced to Cu(I)species,and the activity of the S species is increased after the modification of malachite with ethylenediamine,thus promoting the sulfidization flotation of malachite [16].
In actual mineral processing,metal ions in the pulp are mainly from artificially added flotation reagents,dissolution of associated metal minerals in the crushing and grinding process,and the consumption of grinding medium [1,9,17–21].Different metal ions cause differences in surface properties such as polarity,electricity,and solubility of minerals.Therefore,exploring the effects of metal ions on mineral flotation is very important.Copper ions are common metal ions in pulp;however,few studies have reported the effect of copper ions on mineral sulfidization flotation.Therefore,the effect of copper ion pretreatment on malachite sulfidization flotation was experimentally studied
In this study,the sulfidization flotation behaviour of malachite after copper ion pretreatment was explored through microflotation tests.In addition,the effect of copper ions on collector adsorption on malachite surfaces was determined by contact angle measurements and adsorption tests.The effect of copper ions on the chemical states of Cu and S species on the surface of minerals during sulfidization was analysed using X-ray photoelectron spectroscopy(XPS).Moreover,the copper and sulfur components formed on the mineral surface were visually characterised using time-of-flight secondary ion mass spectrometry (ToF-SIMS) analysis.
2.Experimental
2.1.Mineral samples
Malachite samples were obtained from Guangdong Province,China.A large piece of high-purity malachite was broken apart by hand,washed with deionized water,and air-dried.The pieces of malachite were ground to powder using an agate three-head grinder.The grinder was cleaned with quartz sand and then screened using standard sieves to obtain powder samples with different particle sizes.Powdered samples were labelled appropriately and stored in self-sealing bags for future experiments.Another piece of high-purity malachite was ground to prism shape(8 mm × 8 mm × 2.5 mm) and polished with sandpaper of different particle sizes to obtain the smooth surface.
2.2.Microflotation studies
Microflotation tests were performed using an XFGII flotation machine with a microflotation cell(40 mL).The speed of the flotation machine was set to 1640 r/min.The particle size range of the malachite test minerals was 37–74 μm.For each microflotation test,an accurately weighed 2.0 g sample was used.The pH of the pulp was adjusted using freshly prepared NaOH and HCl solutions.A copper ion solution (CuSO4∙5H2O,Sinopharm Chemical Reagent Co.,Ltd.,Shanghai,China;purity≥99.0%) of the concentration required for the test was added,and the mixture was stirred for 3 min before the Na2S solution (Na2S∙9H2O,Sinopharm Chemical Reagent Co.,Ltd.,Shanghai,China;purity≥98.0%) was added,and the mixture was stirred for another 3 min.The pH of the pulp was recorded with a pH meter,and the pH was adjusted with NaOH or HCl solution.Butyl xanthate (collector) was added at the concentration required for the test,and the mixture was stirred for 3 min.Finally,a known quantity of frother was added.On completion of the flotation,the remaining minerals in the flotation cell and the minerals in the flotation froth were filtered,dried,and weighed to calculate the flotation recovery.
2.3.Contact angle test
Contact angle tests were performed using a JY-82B video contact-angle tester.Pure malachite block samples were used for the test,and the samples were polished before testing.Each sample was placed in deionized water in an ultrasonic bath for cleaning and then dried using an air gun.After the reagent was added to the mineral surface,the sample was quickly transferred to the contact angle tester platform.The contact angle of the mineral surface was measured 3 times for each sample,using the droplet method,and the test results are presented as mean values.
2.4.Zeta-potential measurement
The mineral surface zeta potential value was recorded using a Brookhaven surface zeta potential meter (Brookhaven,Holtsville,NY,USA).The KNO3solution(5×10-3mol/L)was used as the background electrolyte.The malachite powder sample (approximately 0.1 g;particle size less than 5 μm) was transferred to a 100-mL beaker containing KNO3solution and mixed by magnetic stirring.The flotation reagent was added,and the mixture was stirred for 3 min.During stirring,the pH was adjusted with HCl or NaOH solution.The obtained suspension was allowed to stand for 5 min before a disposable pipette was used to extract the supernatant containing fine mineral particles from the upper layer of the suspension.The solution was transferred to the test cell,and the dynamic potential of the mineral surface was measured.Each sample was analysed 3 times,and the results are presented as the mean values.The maximum error did not exceed ±2.0 mV.
2.5.Adsorption experiments
The adsorption capacity of the butyl xanthate collector was tested using ultraviolet visible spectroscopy (UV–Vis) (UV-2700,Shimadzu,Kyoto,Japan).Malachite powder was mixed with the reagents used for the flotation test with variation in the collector concentration,as appropriate.Magnetic stirring was performed throughout the experiments.After flotation,the supernatant was removed from the mixture and centrifuged for 20 min.The resultant supernatant was transferred to a quartz cuvette,and the absorbance at 295 nm was read against a deionized water blank.The collector content adsorbed onto the mineral surface was calculated based on the amount of residual collector detected in the test solution.
2.6.XPS analysis
XPS analysis was performed using a PHI 5000 VersaProbe II spectrometer (ULVAC-PHI,Chigasaki,Japan).X-rays were generated from an aluminium target,and Kα X-rays were used to interrogate the sample (power: 50 W;voltage: 15 kV;pass energy:46.95 eV).Each analysis used approximately 2 g of malachite,and reagents were added successively according to the flotation test conditions.An appropriate volume of deionized water was added to achieve the concentration required for the experiment.Magnetic stirring was performed during the test.After flotation,the samples were filtered and air-dried.Multipak spectral analysis software provided by the instrument manufacturer was used to acquire and analyse the spectra and calculate the elemental content.The energy range of the full-spectrum scan was 0–1200 eV.The spectral data were energy corrected with surface pollution C 1s(284.80 eV)as the standard,and the spectra of other elements were fitted and analysed.
2.7.ToF-SIMS analysis
Mass spectral analysis was performed using a ToF-SIMS V analyser (IONTOF,Münster,Germany).High-purity malachite was ground to the desired shape (8 mm × 8 mm × 2.5 mm) and polished smoothly.Before analysis,the sample was cleaned in an ultrasonic bath and then placed in a beaker to which the required reagents were added.Deionized water was used for dilution,as appropriate,and the sample was soaked for 10 min.The sample was removed from the beaker with tweezers,washed with deionized water,and air-dried.The sample was transferred to the vacuum subchamber and then to the main test chamber when a satisfactory vacuum was achieved.For surface testing,a bismuth gun ion source (30 keV) was used on a test surface of 500 μm × 500 μm,with a test time of 30 s.A bismuth ion source was used for etching,and O2was used for deep sections(1 keV)on a surface area of 300 μm×300 μm,with a test time of 74.75 s.The positive spectrum correction ions were C+,and65Cu+,and the negative spectrum correction ions were CH-,,and Cl-.
3.Results and discussion
3.1.Microflotation study
To investigate the effect of copper ions on malachite sulfidization flotation,we performed microflotation tests with various copper ion concentrations.The tests were performed using 1×10-3mol/L sodium sulfide and 1×10-3mol/L butyl xanthate,and the sulfidization pH was 8.5–9.5.The test results are shown in Fig.1.When the added copper ion concentration was less than 5×10-4mol/L,the flotation recovery increased with increasing copper ion concentration.The highest recovery (70.31%) was observed when the copper ion concentration in the solution reached 5×10-4mol/L.As the copper ion concentration increased further,the recovery of minerals began to decrease,and the recovery was the lowest (17.33%) at a copper ion concentration of 1.5×10-3mol/L.This result indicated that adding a suitable concentration of copper ions improved the recovery of mineral flotation;however,adding a high concentration of copper ions was not conducive to the sulfidization flotation of malachite.After adding a high concentration of copper ions,the concentration of the remaining copper ions in the solution increased.Excess metal ions in the solution consumed flotation reagents,thereby reducing the flotation recovery of malachite.

Fig.1.Malachite flotation recovery as a function of Cu2+ concentrations.
To verify the activation effect of a small amount of copper ion on malachite flotation,we compared the malachite flotation test with and without added copper ions.According to the flotation test results in Fig.1,the flotation test was carried out with the concentration of xanthate as the variable,and the concentrations of Cu2+and Na2S were fixed at 5×10-4and 1×10-3mol/L,respectively.Fig.2 shows that both flotation curves improved as the xanthate concentration increased.This result showed that the floatability of minerals improved as more xanthate ions were adsorbed.After copper ion pretreatment,the flotation recovery was higher than that under direct sulfidization flotation.The highest recovery reached 75.93%,demonstrating that the addition of a small amount of copper ions helped to improve the hydrophobicity of the mineral surface.Therefore,the experimental results of the above flotation(Fig.1) test were proven.

Fig.2.Malachite flotation recovery as a function of xanthate concentrations in the absence and presence of Cu2+.
3.2.Effect of copper ions on the malachite surface hydrophobicity
Contact angle testing is the most intuitive test for determining the hydrophobicity of a mineral surface[22,23].The effect of copper ions on mineral hydrophobicity was assessed by performing a contact angle test at copper ion concentrations of 2.5×10-4and 1×10-3mol/L,and the concentrations of sodium sulfide and xanthate were both 1×10-3mol/L.The contact angle test results are shown in Fig.3.Fig.3a shows the contact angle of malachite after treatment with deionized water and xanthate(62.21°).Because of the strong hydrophilicity of the malachite surface,the contact angle was small.As shown in Fig.3b,the hydrophobicity of the mineral surface after sulfidization was enhanced,and the contact angle increased to 75.18°.After treatment with copper ions at low concentrations(Fig.3c),the contact angle increased slightly to 85.79°.Copper ions acted on the sample surface and increased the number of active sites on the mineral surface,which contributed to the adsorption of xanthate components and increased the hydrophobicity of the mineral surface.Fig.3d shows that pretreatment with a high concentration of copper ions and xanthate reduced the contact angle of the mineral surface to 45.82°,which indicated that the hydrophilicity of the mineral surface improved.At the same time,excess copper ions also consumed collector reagents,which increased the hydrophilicity of the mineral surface.

Fig.3.Contact angles of malachite surfaces under different conditions.
3.3.Effect of copper ions on the malachite surface potential
The metal ions added to the solution are mainly adsorbed at the mineral–solution interface,and this process affects the mineral surface potential.Zeta potential is an important indicator of the mineral-solution interface potential.The adsorption mechanism of ions in the solution on the mineral surface was further analysed using zeta potential testing.As shown in Fig.4a,the isoelectric point of malachite was pH 6.5.When pH<10.5,the potential on the surface of malachite gradually decreased with increasing pH.When pH>10.5,the curve increased slightly,which might have been caused by the increase in the potential on the surface of malachite after the formation of Cu(OH)2under strong alkaline conditions.According to Fig.4b,in the pH range of 6–10,the copper ions in solution mainly exist in the forms of Cu2+,Cu(OH)+and Cu(OH)2(aq/s)[18,24].When copper ions interact with the mineral surface,the mineral isoelectric point shifts to the right,and the potential of the mineral surface increases at pH>6.The experimental results showed that the added copper ions were adsorbed on the surface of malachite to form new copper compounds [Cu2+,Cu(OH)+,and Cu(OH)2] on the mineral surface.The surface potential of malachite pretreated with copper ions decreased significantly after the addition of Na2S,which showed that the negatively charged sulfide might have been adsorbed onto the sample surface after pretreatment with copper ions.After the addition of the collector,the overall trend of the potential curve decreased,which indicated that xanthate ions were on the mineral surface.When the pH was below 7.5 and above 10.5,the potential on the mineral surface was relatively close,which indicated that the collector had poor adsorption on the mineral surface within this range and was not conducive to malachite sulfidization flotation.
3.4.Effect of copper ions on collector consumption on malachite surfaces
The adsorption of the collector on the mineral surface or its consumption in solution was determined by measuring the xanthate concentration in the solution by spectroscopy [1,3,9].Tests were performed with and without copper ion pretreatment.Fig.5 shows the consumption test of butyl xanthate with copper ions added before mineral sulfidization in the case of a decantation solution.Under these conditions,the consumption of sulfur and collector by metal ions was avoided in the solution.The results showed that the consumption of xanthate was the highest without added reagent,which was caused by the dissolution of malachite.After treatment with Na2S,copper sulfide species formed on malachite surfaces,which leads to a decrease in the dissolution of malachite because the solubility of copper sulfide is much less than malachite.Thus,a small quantity of copper ions will be dissolved in the pulp solution after malachite was treated with Na2S,i.e.,the consumption of xanthate species decreased by dissolved copper ions in the pulp solution.After malachite was pretreated with copper ions,the reactive sites on the mineral surface increased,and more copper sulfide species formed on the malachite surface,which greatly decreased the dissolution of malachite and increased the surface stability,so the consumption of xanthate species further decreased.

Fig.4.Zeta potentials of malachite and speciation diagram of various copper-hydroxyl complexes as a function of pH.

Fig.5.Consumption amounts of xanthate as a function of initial xanthate concentrations.
3.5.Effect of copper ion on chemical state of mineral surface elements
XPS can be used for quantitative analysis and structural identification of mineral surfaces,and the valence state of mineral surface elements can be determined using the characteristic binding energies of electrons in the elements of interest [1,9,16,25–28].Therefore,XPS was used to explore the influence of copper ions on the chemical environment of the mineral surface.The atomic concentrations of the malachite samples under different conditions are listed in Table 1.The atomic concentration of copper on the mineral surface of malachite after treatment with deionized water was 13.91%.The addition of 2.5×10-4and 7.5×10-4mol/L Cu2+(samples(b)and(c))increased the atomic concentration of copper to 14.57% and 14.83%,respectively.The atomic concentrations of C 1s and O 1s decreased,indicating that the added copper ions were adsorbed on the surface of the sample and formed coppercontaining components.Sample (d) had atomic concentrations of 3.17%S,12.56%C,65.96%O,and 18.31%Cu on the mineral surface after sulfidization.When malachite was pretreated with copperions,the atomic concentration of S increased to 4.20% and 3.92%,the atomic concentration of O increased to 69.52% and 68.40%,and the other components decreased.This result indicated that the generation of S was increased after pretreatment of malachite with a small amount of copper ions,and the S content decreased after treatment with higher concentrations of copper ions.

Table 1Atomic concentration of malachite samples treated with different reagents.
The XPS spectra of O 1s on the malachite surface under different conditions were analysed.Fig.6a shows the O 1s spectrum of the malachite treatment with deionized water.The two characteristic O 1s peaks at binding energies of 531.32 and 532.28 eV likely corresponded respectively to the O peak of the —Cu—O species and the O peak of hydroxyl groups on the mineral surface (—OH)[1,9].After adding 2.5×10-4mol/L Cu2+,the results are shown in Fig.6b.The binding energies of O shifted to 531.37 and 532.27 eV,which were very small shifts.According to Table 2,the contribution of the hydroxide component on the mineral surface to the total oxygen amount decreased from 41.11% to 35.84%,and the metal—O (—Cu—O) component increased from 58.89%to 64.16%.These results indicate that the main cooper components in the solution were Cu2+,Cu(OH)+,and Cu(OH)2(s)at neutral pH;furthermore,Cu2+binding to the O site of the mineral and a dehydration reaction between Cu(OH)+and —OH increased the copper content on the mineral surface.After treatment with 7.5×10-4mol/L Cu2+,the content of the —OH component on the mineral surface increased to 45.65%,and the content of the metal-O component decreased to 54.35%.According to the literature [16,17],the thickness of Cu(OH)2that forms on the mineral surface usually increases with the increase in the copper ion concentration under medium acidic conditions.Therefore,the higher content of the—OH component on the mineral surface might have been caused by the addition of relatively more copper ions to form Cu(OH)2on the mineral surface.When too much copper hydroxide is adsorbed on the mineral surface,too many hydrophilic groups are on the mineral surface,and then the reaction activity is poor.After mineral surface sulfidization,the binding energies were 531.40 and 532.41 eV.The addition of sulfide ions might have formed the S—O component on the mineral surface,resulting in the shift of the binding energy of—OH component.Compared with the pure mineral surface,the —OH component was greatly reduced,which indicated that the surface hydrophobicity of malachite was increased after sulfidization (Table 2,sample (d)).Compared with that of samples at the sulfidization conditions shown in Fig.6e and f,the binding energy of O on the mineral surface pretreated with different concentrations of copper ions shifted slightly.According to Table 2,after pretreatment with 2.5×10-4mol/L Cu2+,the—OH component on the mineral surface decreased to 28.79% and the —Cu—O component increased to 71.21%.These results suggested that a small addition of copper ions increased the mineral surface activity of the —Cu—O component,making adsorption to the mineral surface by S easier,and significantly decreasing the amount of the hydrophilic —OH component on the mineral surface.This result showed that a small amount of added copper ions increased the hydrophobicity of the sulfide surface,which was conducive to the sulfidization flotation of malachite.After adding 7.5×10-4mol/L Cu2+,the —OH component on the mineral surface increased to 38.73%,which might have been caused by the formation of many Cu(OH)2compounds after the addition of many copper ions.This formation of Cu(OH)2would increase the hydrophilicity of the mineral surface and would not be conducive to the subsequent adsorption of S and collectors.

Fig.6.O 1s XPS survey spectra of malachite treated with different conditions.

Table 2Binding energy,percentage in total O of different O species on malachite after treated with different reagents.
Fig.7 shows the effect of copper ion addition on Cu on the surface of malachite.The double peaks of Cu 2p in the XPS spectrum had single symmetry,so the chemical properties of the Cu 2p1/2and Cu 2p3/2characteristic peaks are the same[3,10,14].As shown in the spectra of the pure malachite surface (Fig.7a),Cu 2p3/2had binding energy peaks at 935.00 eV,respectively.Because of the Cu—OH group on the malachite surface,two satellite peaks appeared next to each of these peaks,which indirectly proved the purity of the mineral.After adding 2.5×10-4mol/L Cu2+(Fig.7b),the binding energy of Cu 2p3/2shifted from 935.00 to 934.79 eV,with a binding energy shift to the left of 0.21 eV.The added copper ions possibly formed new copper components(such as—Cu—O)on the malachite surface,which would have an activation effect on the mineral surface.After treatment with 7.5×10-4mol/L Cu2+,the binding energy on the mineral surface shifted to 934.99 eV (Fig.7c).With the addition of a relatively high concentration of copper ions,copper ions also formed many Cu—OH groups on the mineral surface,which is not conducive to the malachite sulfide flotation.As shown in the Cu 2p XPS spectra in Fig.7d,the Cu 2p3/2binding energies after sulfidization of the copper sulfide(Cu2S)and the copper components of the mineral were respectively 932.88 and 935.07 eV.After copper ion pretreatments at different concentrations before sulfidization (Figs.7e and f),the binding energy of Cu(I) on the mineral surface shifted to 933.08 and 933.25 eV.This shift might have been caused by the chemical reaction between copper and sulfur ions which formed Cu—S.The chemical environment of the Cu—S component on the mineral surface changed,and the binding energy shift of the Cu(II)component was small,indicating that these groups had little effect on the copper component of malachite.According to Table 3,after pretreatment with 2.5×10-4mol/L Cu2+,the Cu(I) component on the mineral surface increased to 34.70%,which meant that —Cu—O adsorbed on the mineral surface easily reacted with S,resulting in an increase in the amount of Cu—S on the mineral surface.This increase would promote the sulfidization effect and further improve the floatability of the mineral.After adding 7.5×10-4mol/L Cu2+,the Cu(I) component on the mineral surface decreased to 27.40%,which indicated that the proportion of the Cu—S component on the malachite surface of the total amount of copper decreased after the addition of a high concentration of copper ions.Many copper hydroxide groups (72.60%) were adsorbed on the sample surface,resulting in a reduction of the reaction activity of the sulfidization products.Therefore,we inferred that a small amount of copper ions had an activation effect on malachite,whereas the addition of excessive copper ions was not conducive to the enrichment and recovery of malachite.

Table 3Binding energy,percentage in total Cu of different Cu species on malachite after treated with different reagents.

Fig.7.Cu 2p XPS spectra of malachite treated with different conditions.
3.6.ToF-SIMS study
ToF-SIMS analysis provides surface analysis and deep profile detection of elements on mineral surfaces.Surface analysis detects the signal strengths of positive and negative ions on the mineral surface.Deep profile testing can intuitively test the adsorption layer formed by agents or ions on the mineral surface [1,9,29].Fig.8 compares the ToF-SIMS two-dimensional(2D)spectra of copper ions on the mineral surface under different conditions.Given that Cu2+are the main metal element in malachite,many Cu+signals were detected on the pure malachite surface(TC:1.596×105).After the addition of 5×10-4mol/L copper ions,the strength of the Cu+signal on the malachite surface increased (TC: 2.399×105),probably because the added copper ions were adsorbed on the malachite surface.According to the above experimental results,the adsorption of copper ions on the mineral surface was conducive to the subsequent adsorption of S species.

Fig.8.2D distribution of Cu+ species and positive-ion depth profile for malachite samples treated with different conditions.
To determine whether copper ions produce an adsorption layer on malachite,we conducted a deep profile analysis test on the mineral surface using an O2ion source,and the results are shown in Fig.8.Because copper ions are the dominant metal ion of malachite,the signal intensity of Cu+was higher than that of CuO+(Fig.8a) when no metal ions were added.With increasing etching time,the change in the Cu+signal intensity on the mineral surface was slight,which indicated that the detected copper ion signal might have been the Cu+signal of the mineral.As shown in Fig.8b,after copper ions acted on the mineral surface,there was a large gap between the copper ion signal on the mineral surface with increasing etching time,and the copper ion signal on the mineral surface tended to increase.Therefore,combined with the surface analysis results of Fig.8 and the results of this etching analysis,we speculate that copper ions were adsorbed on the surface of malachite and formed an adsorption layer of copper ions.

Fig.9.2D distribution of ions on malachite surfaces treated with different conditions.

Fig.10.Negative-ion depth profile for malachite samples treated with different conditions.

Fig.11.3D distribution of S- and species on malachite surfaces treated with different conditions.
We used ToF-SIMS to analyse the surface and deep profile of malachite samples with added Cu2+before sulfidization,in which the concentration of Cu2+was 5×10-4mol/L and the Na2S concentration was 1×10-3mol/L.Fig.9 shows the occurrence of Cu+and S-on the surface of malachite.With no addition of copper ions,the copper ion signal was from malachite (Fig.9a).After the mineral was pretreated with copper ions,the ion distribution diagram of sulfidization samples (Fig.9b) showed that the signal for S-was enhanced.This result showed that the content of sulfide products after copper ion pretreatment was enhanced.The signal for copper ions on the mineral surface was weakened,which might have been caused by the increased amount of S species covering the mineral surface.
The deep etching test results are shown in Figs.10 and 11.When the malachite surface was pretreated with copper ions and sulfidization (Fig.10b),the signal intensity of S-coincided with that of the bulk ion when the etching time was 47.5 s,and the intensity ofwas lower than that ofafter 8 s.Compared with that of the surface of malachite after direct sulfidization,the etching time shifted significantly.This result showed that the sulfide layer of the sample became thicker after copper ion treatment.Therefore,the addition of a certain amount of copper ions before sulfidization effectively promoted the adsorption of sulfur ions.The three-dimensional (3D) distribution of S-andfrom the etching test is shown in Fig.11.The sulfur component signal of the malachite sample treated with copper ions was enhanced compared with that of the malachite sample subjected to sulfidization.This result showed that copper ion treatment can promote the adsorption of S on the mineral,which increased the thickness of the sulfide layer on the malachite surface.
4.Conclusions
In this study,we investigated the adsorption of copper ions in solution onto the surface of malachite.The results helped to clarify the mechanism of malachite sulfidization after pretreatment with copper ions.Based on the experimental results,the main conclusions are drawn as follows.
(1) According to the results of microflotation and contact angle testing,after pretreatment of the malachite surface with a low copper ion concentration,the recovery of mineral sulfidization flotation was improved.However,the floatability of malachite was depressed after pretreatment with a high concentration of copper ions.The collector adsorption test indicated that the pretreatment of copper ions was helpful in reducing the consumption of xanthate by malachite dissolution.
(2) XPS and zeta potential analysis results indicated that copper species can be chemisorbed on the malachite surfaces.The amount of the sulfide product Cu—S increased,and the activity of sulfide products on the mineral surface improved after pretreatment with a low copper ion concentration.Conversely,the Cu—(OH)2component was the dominant component on the mineral surface after the addition of a high concentration of copper ions,which was not conducive to the sulfidization of malachite.
(3) ToF-SIMS analysis indicated that the addition of copper ions increased the number of active sites for the subsequent adsorption of S,and the thickness of the sulfide layer on the mineral surface increased.
Acknowledgments
This work was supported by Yunnan Fundamental Research Projects (No.202101BE070001-009),Open Foundation of State Key Laboratory of Mineral Processing (No.BGRIMM-KJSKL-2021-24),and Ten Thousand Talent Plans for Young Top-notch Talents of Yunnan Province (No.YNWR-QNBJ-2018-051).
杂志排行
矿业科学技术学报的其它文章
- Effect of deep oxidation of chalcopyrite on surface properties and flotation performance
- Insights into the adsorption performance and mechanism of hydrated Ca ion on talc (001) basal surface from DFT calculation
- Effect of bastnaesite as reductant on hematite reduction during in-situ suspension magnetization roasting of refractory iron ore under neutral atmosphere
- Application of multi-stage dynamic magnetizing roasting technology on the utilization of cryptocrystalline oolitic hematite: A review
- A review of flotation and selective separation of pyrrhotite:A perspective from crystal structures
- Influences of different modifiers on the disintegration of improved granite residual soil under wet and dry cycles