Influences of POSS-E-GO Content on Mechanical Properties of Bio-based Epoxy/DOPO-POSS Nanocomposites

2022-07-13DUYonggangSHIGonghuiWANGJiamingWANGYimingWANGXuhuaWANGLiweiYANGJinhuiRENShitong

DU Yonggang, SHI Gonghui, WANG Jiaming, WANG Yiming, WANG Xuhua,WANG Liwei, YANG Jinhui, REN Shitong

(1. School of Materials Science and Engineering, Shijiazhuang Tiedao University, Shijiazhuang 050043, China; 2. Hebei Key Laboratory of Advanced Materials for Transportation Engineering and Environment, Shijiazhuang 050043, China)

Abstract: The bio-based epoxy nanocomposite (GAER/DOPO-POSS) was prepared from gallic epoxy resin (GAER) and polyhedral oligomeric silsesquioxane (which containing 9,10-dihydrogen-9-oxo-10-phosphorus-phenanthrene-10-oxide groups, called DOPO-POSS). The polyhedral oligomeric silsesquioxane containing epoxy groups (E-POSS) was grafted onto aminated graphene oxide (E-GO), then the novel POSSE-GO was obtained. The POSS-E-GO was used as modifier for GAER/DOPO-POSS nanocomposite. The influences of POSS-E-GO content on mechanical properties, dynamic mechanical properties and thermal stability of GAER/DOPO-POSS nanocomposites were determined. The experimental results show that POSS-E-GO can significantly improve the toughness of the GAER/DOPO-POSS nanocomposite. When 0.5wt% POSS-E-GO was added in GAER/DOPO-POSS nanocomposite, the impact strength of the nanocomposite was 4.74 kJ/m2 higher than that in the absence of POSS-E-GO, meantime the initial thermal degradation temperature was 277 ℃.

Key words: epoxy resin; impact resistance; nanocomposites

1 Introduction

Epoxy resin has excellent bonding properties, electrical insulation properties, chemical resistance, and low manufacturing costs. Therefore, epoxy resin has been widely used in automotive, aerospace, electrical industries, adhesives, coatings and other fields. At present, epoxy resin mainly derives from petrochemical products, of which more than 80% are based on di-glycidyl ether of bisphenol A (DGEBA). Thus, it is of important scientific and environmental value to find renewable plant resources which can replace petrochemical products to prepare epoxy resin with high-performance.

A large number of studies on bio-based epoxy resins have been reported, including epoxy resins based on vegetable oil, natural polyphenols, carbohydrate, lignin, and some other biomass. The earliest developed bio-based epoxy resins are mainly derived from vegetable oil. However, due to the existence of aliphatic branches and low epoxy value, this kind of cured epoxy resin is often found to have defects such as poor water resistance, heat resistance and mechanical strength. Hence, many scholars have focused on biomass matrix which containing rigid structure to synthesize epoxy resins, such as rosin, eugenol, daidzeinand furfural,

etc

. These results indicate that rigid epoxy resins with appropriate cross-link density have good mechanical properties and thermal stability.Gallic acid is a natural polyphenol, widely found in rhubarb, eucalyptus, cornus and other plants. Gallic acid has a wide range of applications in food, biology, medicine, chemical industry and other fields. Gallic acid contains three phenolic hydroxyl groups and one carboxylic group which can be exploited in order to obtain bio-based epoxy resin with improved thermal and mechanical properties. Aouf

et al

synthesized gallic epoxy matrix by two steps of allylation and oxidation. Compared with DGEBA, gallic epoxy resin has higher carbon residue and glass transition temperature. The results of our previous work indicated that the impact strength of pure gallic epoxy resin was 1.42 kJ/mhigher than that of DGEBA. Therefore, gallic acid is expected to be an alternative biomass to bisphenol A to prepare high-performance epoxy resin.

Bio-based epoxy resins also have the disadvantages of brittleness. In recent years, nano modifiers based on polyhedral oligomeric silsesquioxane (POSS) and graphene have attracted widespread attention. It is well known that graphene with good dispersibility in polymer matrix can significantly improve the mechanical properties of materials. The PPA-g-GNS was obtained by grafting polyphosphate amide onto graphene sheet by Wangand used as modifier for DGEBA. The results showed that the grafted molecular chain could prevent the restacking of graphene. The flame retardancy of DGEBA was significantly improved with the addition of PPA-g-GNS, but the mechanical properties of DGEBA were negatively affected.

POSS is based on inorganic silica skeleton, which retains excellent thermal stability and mechanical properties of inorganic materials. When POSS undergoes thermal degradation, a dense silica protective layer can be formed, thereby delaying the thermal degradation process of the material. POSS has good application prospects in improving the mechanical properties and thermal stability of polymers. Zhang

et al

used DOPO-POSS (which terminal groups are 9,10-dihydrogen-9-oxo-10-phosphorus-phenanthrene-10-oxide) as modifier for DGEBA, and found that the carbon residue rate of the epoxy resin was improved. Meantime, the cone-shaped calorimetry test results showed that the flame retardance of the modified epoxy resin was significantly improved. From our previous work as mentioned above, we found that the compatibility of DOPO-POSS with gallic epoxy was not good. Only when the content of DOPO-POSS was not more than 6%, DOPO-POSS could improve the impact strength and flame retardancy of epoxy resins at the same time. However, the impact strength of GAER/DOPO-POSS needs to be further improved.

In this article, POSS-E-GO was synthesized by grafting E-POSS onto aminated graphene oxide, which combines the advantages of graphene and POSS. POSS-E-GO was used as modifier for GAER/ DOPO-POSS nanocomposites. The influences of POSSE-GO content on mechanical properties, dynamic mechanical properties and thermal stability of GAER/DOPO-POSS nanocomposites were discussed.

2 Experimental

2.1 Materials

Gallic acid (supplied by Tianjin Yongda Chemical Reagent Co. Ltd, China), epichlorohydrin and ethylenediamine (supplied by Tianjin Fuchen chemical Reagent Factory, China), N,N-Dimethylbenzylamine and graphite powder (supplied by MacLean Biochemical Technology Co. Ltd, China), isopropanol and methacrylic acid (supplied by Tianjin Kemeiou Chemical Reagent, Ltd, China ), KH-560 (supplied by Nanjing Chengong Silicone Material Co., Ltd, China ), maleic anhydride (supplied by Tianjin Baike Chemical Reagent Co., Ltd, China ), triphenylphosphine (supplied by Sain chemical Technology Co., Ltd, China), 9,10-dihydro-9-oxo-10-phosphorus-phenanthrene-10-oxide (supplied by Shanghai Aladdin Reagent Co., Ltd, China).

2.2 Synthesis of gallic epoxy resin

A mixture of gallic acid (0.10 mol), epichlorohydrin (2.20 mol) and cetyltrimethylammonium bromide (0.007 mol) was heated to 100 ℃ and stirred for 6 h. Then the mixture was cooled to 50 ℃, 0.44 mol sodium hydroxide was gradually added into the mixture and reacted for another 1 h at 70 ℃. After that, the mixture was washed by deionized water to neutral, and dried by magnesium sulfate for 12 h. After the residual epichlorohydrin was removed under vacuum condition, a yellow viscous liquid was obtained. The epoxy value of gallic epoxy resin was determined by hydrochloric acid-acetone titration. The measured epoxy value of gallic epoxy resin is 0.75 (theoretical value is 1.02).

2.3 Synthesis of DOPO-POSS

E-POSS was synthesized according to our previous work. A mixture of E-POSS (0.10 mol), DOPO (0.80 mol) and triphenyl phosphine (0.025 mol) was dissolved in 100 mL toluene and added to a 250 mL flask. The mixture was stirred at 120 ℃ for 2 h, then toluene was removed under vacuum condition. After that DOPO-POSS was obtained and dried at 60 ℃ in oven for 6 h, then dried in a vacuum oven at 40 ℃ for 24 h. The synthetic route of DOPO-POSS is shown in Fig.2.

Fig.2 Synthetic route of DOPO-POSS

2.4 Synthesis of POSS-E-GO

Graphene oxide (GO) was synthesized by improved Hummer’s method. A mixture of 0.3 g GO and 300 mL·N, N-dimethylformamide (DMF) was added to a 500 mL beaker and treated with ultrasound for 50 min. After that the mixture was poured into a 500 mL four-necked flask equipped with thermometer, spherical condenser, constant pressure dropping funnel, and stirring device. Then 2.7 g ethylenediamine was added dropwise to the flask within half an hour, and the mixture was stirred at 90 ℃ for 8 h. After the reaction, the black precipitate was obtained by high-speed centrifugation and washed by methanol for three times. Finally, E-GO was obtained by freeze-drying.

A mixture of 0.4 g E-GO and 300 mL DMF was added to a 500 mL beaker and treated with ultrasound for 40 min. Then the mixture was poured into a 500 mL flask. 0.8 g E-POSS was added in the mixture, then the mixture was stirred at 70 ℃ for 12 hours. After the reaction, the black precipitate was obtained by highspeed centrifugation and washed by deionized water for three times. Finally, POSS-E-GO was obtained by freeze-drying. The synthetic route of POSS-E-GO is shown in Fig.3.

Fig.3 Synthetic route of POSS-E-GO

2.5 Preparation of bio-based epoxy nanocomposites

The composition of each sample is shown in Table 1. Maleic anhydride was used as curing agent for epoxy resin. The raw materials in various proportions were mixed evenly and dispersed in acetone, then the mixture was poured into preformed model. After that, acetone was removed in a vacuum oven at 45 ℃ for 1 h. The curing reaction was performed at 80 ℃ for 2 h,130 ℃ for 3 h, and 150 ℃ for 2 h. Sample P is pure gallic epoxy resin as a reference sample. All the matrix of A0-A5 are GER/DOPO-POSS, and DOPO-POSS content is 6% of the mass of gallic epoxy resin. In samples A1-A5, the contents of POSS-E-GO are 0.1%, 0.2%, 0.3%, 0.4%, and 0.5% of the mass of gallic epoxy matrix, respectively.

Table 1 Sample composition

Sample number Gallic epoxy resin/g POSS-E-GO/g DOPO-POSS/g Maleic anhydride/g P 17.65 0 0 6.22 A0 17.65 0 1.07 6.22 A1 17.65 0.018 1.07 6.22 A2 17.65 0.035 1.07 6.22 A3 17.65 0.053 1.07 6.22 A4 17.65 0.071 1.07 6.22 A5 17.65 0.088 1.07 6.22

2.6 Measurements

The infrared spectroscopy of DOPO-POSS and POSS-E-GO were determined by a Nicolet-310 (Thermo Electron Corporation, USA) using transmission mode. Impact strength test referred to ASTM D6110-2010 for sample preparation and testing. The impact section morphology of each sample was measured by a HITACHI SU8010 scanning electron microscope (Hitachi, Japan). Dynamic mechanical properties of samples were determined by DMA-8000 (PE Corporation, USA). All the samples were heated from 25 to 170 ℃ with a heating rate of 2 ℃/min. The testing mode was single-cantilever vibration, and the testing frequency was 2 Hz. The limiting oxygen index of each sample was determined by an FTAII oxygen index meter (RC, Corporation, UK) according to ASTM D2863-2008. Thermogravimetric analysis (TGA) was determined by TGA-4000 (PE Corporation, USA). All samples were heated from room temperature to 800 ℃ under nitrogen atmospheres with a heating rate of 20 ℃/ min.

3 Results and discussion

3.1 Infrared spectra analysis

As seen from Fig.4, the peaks at 2 437, 1 596, 1 473, 1 230, and 948 cmcorrespond to P-H, benzene ring skeleton, P-Ph, P=O, and P-O-Ph stretching vibration of DOPO, respectively. The characteristic peaks at 2 935 and 2 866 cmbelong to -CH. The characteristic peaks at 1 345, 1 108, and 912 cm, correspond to C-O-C, Si-O-Si, and epoxy group, respectively. These are the characteristic peaks of the unique functional group of E-POSS. DOPO-POSS has the characteristic peaks of -CH, benzene ring skeleton, P-Ph, P=O, Si-O-Si, and P-O-Ph. In addition, DOPO-POSS has a hydroxyl peak at 3 313 cm, which is generated by the ring-opening reaction between the epoxy group of E-POSS and the P-H bond of DOPO. The measured epoxy value of DOPO-POSS is 0, indicating that there are no residual epoxy groups in DOPO-POSS. Therefore, it can be proved that DOPO-POSS is successfully synthesized.

Fig.4 Infrared spectra of DOPO-POSS

The infrared spectra of E-GO and POSS-E-GO are shown in Fig.5. The characteristic peaks at 2 970 and 2 835 cmbelong to -CH. The peak of hydroxyl stretching vibration appears at 3 250 cm. The peaks at 1 602 and 1 066 cmcorrespond to C=C and C-O, respectively. These characteristic peaks of E-GO are similar to those reported in the Ref.[35]. In addition to E-GO characteristic peaks, POSS-E-GO also contains stretching vibration peaks of Si-O-Si and epoxy group, which appear at 1 104 and 914 cm, respectively. These evidences indicate that POSS-E-GO is successfully synthesized.

Fig.5 Infrared spectra of POSS-E-GO

3.2 X-ray diffraction analysis

With the aim of detecting the variations of the layer structure among the samples, an XRD analysis was performed, and the patterns are depicted in Fig.6. The characteristic peak of natural graphite (NG) appears at 26.60°, and the corresponding interlayer distance is 0.334 nm. After oxidation and amination, the characteristic peak of E-GO appears at 10.04°, and the corresponding interlayer distance is 0.880 nm. Due to various residual oxygen-containing groups and grafted ethylenediamine, the interlayer spacing of E-GO increased. There are almost no characteristic peaks belonging to POSS-E-GO, because the regular structure of E-GO is further destroyed after E-POSS grafting.

Fig.6 XRD patterns of different samples

3.3 Transmission electron microscopy analysis

TEM images of GO, E-GO, and POSS-E-GO are shown in Fig.7. As seen from the image, a large single-layer GO sheet can be observed clearly. This indicates that the oxidation reaction is relatively thorough and the lamellar structure is completely peeled off. At the same time, it can be seen that there are wrinkles and curls on the edge of the sheet, which is a defect formed during the oxidation process. One amine group of ethylenediamine can react with epoxy groups or carboxyl groups on the graphene oxide sheet, which is beneficial to the peeling of the sheet structure. A large single-layer sheet of POSS-E-GO can be observed. The terminal groups of E-POSS are epoxy groups, which can undergo ring-opening reactions with the amine groups on the E-GO sheet, thus the E-POSS can be grafted onto the E-GO sheet. The black spheroids on the sheet are grafted E-POSS molecules. It can be seen from the figure that the grafted spheroids are dispersed. The restacking of aminated graphene oxide sheet is effectively prevented by the grafting of E-POSS. This phenomenon is an evidence of the XRD results discussed above. However, it is not excluded that there are a small number of stacked structures in some areas.

Fig.7 TEM images of GO, E-GO, and POSS-E-GO

3.4 Mechanical properties analysis

The impact strength of each sample is shown in Fig.8. The impact strength of sample A0 (GAER/DOPO-POSS) is 0.30 kJ/mhigher than that of sample P (pure GAER). This is because that DOPO-POSS is a rigid molecule with large steric hindrance effect. When subjected to external force, DOPO-POSS can induce craze and absorb impact energy. It should be noted that the toughening effect of DOPO-POSS on GAER is not ideal, so the mechanical properties of GAER/DOPO-POSS composites need to be further improved. As seen from Fig.8, the impact strength of A series samples increases with increasing POSS-E-GO content. When the POSS-E-GO content is 0.5%, the impact strength of sample A5 is 4.67 kJ/mhigher than that of sample A0 (without POSS-E-GO). This shows that POSS-E-GO can significantly improve the mechanical properties of GAER/DOPO-POSS composites. This is due to the grafting of E-POSS to the E-GO sheet prevents the restacking of the E-GO sheet, thus showing a good toughening effect.

Fig.8 Impact strength of each sample

3.5 Scanning electron microscopy analysis

The impact cross-section images of different samples are shown in Fig.9. The cross section of sample A0 is rougher than that of sample P, reflecting the toughening effect of DOPO-POSS on GAER. Meantime, it should be noted that there are a few particles on the cross section of sample A0. As mentioned above, when the content of DOPO-POSS exceeds 6%, the compatibility of the composite will deteriorate. The section of sample A3 has the characteristics of ductile fracture, and there is no particle on the surface. The POSS-E-GO terminal groups contains epoxy groups, which makes POSS-E-GO compatible with the GAER matrix and can participate in the curing reaction of GAER matrix. POSS-E-GO and DOPO-POSS have similar molecular structures, so they are partially compatible. It seems that POSS-E-GO plays a role of compatibilizer for GAER/DOPO-POSS composite. However, when the POSS-E-GO content is increased to 0.5%, the compatibility of the nanocomposite is still not good. The cross section of sample A5 is similar to that of A0, and some of particles are observed, too.

Fig.9 SEM images of different samples

3.6 Dynamic mechanical analysis

The tan

δ

and storage modulus of each sample are shown in Fig.10. As seen from the figure, each sample has only one internal friction peak. There is a one-toone relationship between the temperature

T

(which corresponding to the maximum of internal friction peak) and the glass transition temperature

T

.

T

is generally regarded as

T

of polymers. On the basis of the rubber elasticity theory, the crosslink density (

V

) could be obtained from the plateau of the elastic modulus in rubbery state. The

T

and

V

of samples are shown in Table 2.

Fig.1 The graphical abstract of this article

Fig.10 Tanδ and storage modulus of different samples

Table 2 and of each sample

Sample number P A0 A1 A2 A3 A4 A5 Tg /℃ 108.8112.2118.5117.5123.4118.9114.2 Ve / (kmol/m3) 6.17 5.37 7.95 8.74 7.65 7.42 6.27

The

T

of sample A0 is 3.4 ℃ higher than that of sample P. This is because the addition of DOPO-POSS increases the rigidity of the material. At the same time, DOPO-POSS has obvious steric hindrance effect, and it has no functional group which can react with matrix, thus the

V

of sample A0 is lower than that of sample P. The epoxy groups contained in POSS-E-GO molecule can participate in the curing reaction of matrix. Thus, both the

T

and

V

increase with increasing POSS-EGO content. As mentioned in the SEM analysis, when the content of POSS-E-GO is higher than 0.3%, the compatibility of the material becomes poor, resulting in a slight decrease in

T

and

V

, but still higher than that of A0.

3.7 Thermal gravimetric analysis

The thermal degradation curves of different samples are shown in Fig.11. As shown in the figure, the mass residual rate of sample A0 is the highest among all samples at the same temperature. The thermal stability of every sample which containing POSS-E-GO is lower than that of sample A0 (without POSS-E-GO). This is because the POSS-E-GO molecule contains hydroxyl groups, which will dehydrate when the material is heated. The thermal stability of nanocomposites increases with increasing POSS-E-GO content. POSSE-GO combines the advantages of graphene and POSS. The graphene sheet has a barrier effect, which can delay the heat and oxygen contact between the material and the outside. In addition, graphene has good compatibility with the carbon layer formed during the thermal degradation of the material, which can improve the strength of the carbon layer. On the other hand, when POSS undergoes thermal degradation, a dense silica protective layer can be formed, thereby delaying the thermal degradation process of the material. When the POSS-E-GO content is 0.5%, the initial thermal degradation temperature

T

of the sample is 277 ℃.

Fig.11 Thermal degradation curves of each sample

4 Conclusions

A novel nano-modifier POSS-E-GO was synthesized in this article. The grafted E-POSS effectively prevented the restacking of the aminated graphene oxide sheet, and made the POSS-E-GO compatible with the epoxy resin. POSS-E-GO can significantly improve the impact strength of the GAER/DOPO-POSS nanocomposite. POSS-E-GO can be used as an efficient impact modifier for epoxy resins.