Synergistic Effect of Ta2O5/F-C Composites for Effective Electrosynthesis of Hydrogen Peroxide from O2 Reduction①
2021-03-15WANGKePANGYongYuXIEHuanSUNYuanCHAIGuoLiang
WANG Ke PANG Yong-Yu XIE Huan SUN Yuan CHAI Guo-Liang②
a (College of Chemistry and Materials Science, Fujian Normal University, Fuzhou 350007, China)
b (State Key Laboratory of Structural Chemistry, Fujian Institute of Research on the Structure of Matter, Chinese Academy of Sciences, Fuzhou 350002, China)
ABSTRACT The electrosynthesis of H2O2 as an environmentally friendly green process has attracted great attention due to the importance of H2O2 in industry and human lives. In this work, a new strategy was proposed to improve the electrical conductivity and H2O2 selectivity of transition metal oxides catalysts. F-C (F doped carbon)was coupled with Ta2O5 by calcining polyvinylidene fluoride (PVDF) as the carbon source using one step method.The Ta2O5/F-C composite catalysts show an excellent H2O2 selectivity of more than 80% as well as high reactivity at 2.52 mA/cm2, which is greatly enhanced compared to the counterparts of F-C (selectivity of 59%) and Ta2O5-800(current density of 0.85 mA/cm2) in 0.1 M KOH solution. The onset potential for H2O2 production on Ta2O5/F-C composites is 0.78 V in 0.1 M KOH, which indicates a negligible overpotential. In addition, H2O2 selectivity of the catalyst can be stabilized at more than 80% after 10 hours of electrolysis in alkaline electrolyte. The high performance due to the introduction of F-C increases the conductivity of Ta2O5 and the synergistic effect between F-C and Ta2O5.This work proposed an efficient synergistic effect among F-doped C and Ta2O5 for H2O2 production.
Keywords: Ta2O5/F-C, oxygen reduction reaction, hydrogen peroxide;
1 INTRODUCTION
Hydrogen peroxide (H2O2) is one of the 100 most important chemicals in the world[1]. Because of its strong oxidative properties and the only by-product is water[2,3],H2O2as a green oxidant is often used in almost all chemical industry fields, such as medicine, chemical synthesis,environmental protection, paper bleaching, disinfection,water treatment and so on[2,4-7]. So far, 95% of the total H2O2productions annually comes from the anthraquinone process(AO), which contains a multi-step complex process such as hydrogenation over Pd catalyst and rapid oxidation by O2to generate H2O2[3,8-10]. However, such AO process needs complicated steps and several side reactions which cause unnecessary energy consumption[9,11]. Secondly, the extremely poor stability of high-concentration H2O2poses safety hazard and high transportation costs[12]. Therefore, the development of low-cost and low-concentration H2O2synthesis methods has received increasing attention[5]. One alternative process is the direct synthesis of H2O2from H2and O2with a noble metal alloy catalyst[13-15]. However, this process is not only inefficient but also has a risk of explosion due to the hydrogen-oxygen mixture[12]. Another alternative is photocatalytic production of hydrogen peroxide from water and dioxygen[16,17]. Nevertheless, this method also has the disadvantages of slow kinetics and low efficiency[1,2].Recently, electrosynthesis of H2O2via two-electron O2reduction replacing the AO process has caused more and more attention because it is a green process that is efficient,energy-saving and safe[2,18].
Due to its low price and abundance, transition metal oxides(such as MnO2, Co3O4, Fe3O4, V2O5, Ta2O5and so no) have been widely used as an alternative to precious metals in electrocatalytic oxygen reduction reaction (ORR) catalysts[19-24]. In general, metal oxides show limited ORR performance due to poor electronic conductivity and agglomeration issues[25].
Ta2O5is currently used as an efficient ORR catalyst due to its high oxygen reduction onset potential (~0.95 V vs. SHE)and excellent stability under corrosive environments[26-28].However, the limited electronic transport of Ta2O5always reduces its kinetic reaction rate[29]. Recently, Ta2O5was found to be an efficient catalyst for two electrons ORR to generate H2O2[24,26]. Carbon supports (such as Vulcan XC72R (V),printex L6 (P)[22,30], RGO[31], carbon black[32], etc.) show good conductivity and large surface areas have been proved to be helpful to improve the electronic transport and catalytic activity of metal oxides.
Herein, a simple and effective strategy has been proposed to improve the catalytic activity and electronic conductivity of Ta2O5for H2O2electrosynthesis. The polyvinylidene fluoride (PVDF) has been carbonized to high surface area F doped porous carbon and coupled with Ta2O5nanospheres by a simple calcination to generate Ta2O5/F-C composite. The Ta2O5/F-C composite catalyst presents an excellent performance for H2O2generation with H2O2selectivity and achieves more than 80% and negligible overpotential in 0.1 M KOH alkaline solution, which is greatly enhanced compared to the counterparts of F-C and Ta2O5. The enhanced performance was attributed to the synergistic effect between F-C and Ta2O5, which increases the conductivity of Ta2O5and improves the selectivity of H2O2.
2 EXPERIMENTAL
2. 1 Materials
Potassium hydroxide (98.5%) and tantalum powder (99.9%)were bought from Aladdin company. Hydrofluoric acid(40%), nitric acid (65~68%), ammonium hydroxide (25~28%), N-methylpyrrolidone (NMP, 99%), monopotassium phosphate (99.5%) isopropanol (99.7%), glucose (AR) and dipotassium phosphate (99%) were gotten from Sinopharm Chemical Reagent Co. Ltd. PVDF (HSV900) was bought from HeiFei-kejing. Nafion solution (5%) is gotten from Shanghai Hesen Electric Co. Ltd.
2. 2 Synthesis of Ta2O5 sphere precursor
The Ta2O5sphere precursor was prepared by a co-precipitation process in a typical previous synthesis procedure[33].First, 11 mL HF, 22 mL HNO3and 77 mL deionized water were mixed and then 1 g tantalum powder was carefully poured into the above solution. Ta powder is completely dissolved after six hours. Finally, a certain amount of ammonium hydroxide was injected to the solution and a white precipitation was generated. The white precipitates were separated, washed with deionized water for three times and then dried in an oven at 60 ℃ overnight to obtain the final products of Ta2O5nanospheres.
2. 3 Synthesis of Ta2O5/F-C, Ta2O5-800 and F-C
Ta2O5/F-C was prepared using one-step process. 0.1 g PVDF and 0.1 g Ta2O5nanospheres were milled with a mortar for 30 minutes, then a certain amount of NMP as a binder was added during the milling process. Such viscous colloids were dried overnight in an oven at 60 ℃ and then calcinated in a tube furnace at 800 ℃ for 2 h with a heating rate of 5 ℃/min in N2. Then, they were cooled down to room temperature naturally. The black powders were generated and marked as Ta2O5/F-C. As a comparison, PVDF and Ta2O5nanospheres with a mass ratio of 1:2 and 2:1 were also treated with the same process. The products were marked Ta2O5/F-0.5C and Ta2O5/F-2C, respectively. 0.1 g PVDF was calcinated in a tube furnace at 800 ℃ for 2 h at a heating rate of 5 ℃/min in N2and marked as Ta2O5-800. 0.1 g Ta2O5nanosphere calcinated in a tube furnace at 800 ℃ for 2 h with a heating rate of 5 ℃/min in N2was marked as F-C.
2. 4 Structure characterization
The transmission electron microscopy (TEM) images were obtained by using JEOL field-emission microscope (JEOL,Tokyo, Japan) operated at 200 kV. A field emission scanning electron microscope (SEM, FESEM, JSM6700F) equipped with an energy dispersive X-ray spectroscope (EDX, Oxford INCA) is used for acquired SEM images and collecting EDX data (Random five points). X-ray diffraction (XRD) patterns were captured by Miniflex 600 X-ray diffractometer under CuKα radiation. X-ray photoelectron spectroscopy (XPS)was recorded on an ESCALAB 250Xi X-ray photoelectron spectrometer (Thermo Fisher) using monochromatized AlKα radiation (15 kV, 10 mA). The specific surface areas were measured using the Brunauer-Emmett-Teller (BET) model.
2. 5 Electrochemical measurements
All electrochemical measurements were performed by an electrochemical workstation (Autolab, PGSTAT302N).Linear sweep voltammetry (LSV) and cyclic voltammetry(CV) experiments were performed using a single cell on a three-electrode system including a platinum gauze as the counter electrode, a saturated Ag/AgCl electrode as a reference electrode and a rotating ring-disk electrode (RRDE,the areas of ring and desk electrodes are 0.07212 and 0.19625 cm2) as working electrode. The H2O2selectivity was acquired by RRDE experiments in oxygen saturated electrolyte (two electrolytes with pH~8 (phosphate buffered saline) and pH~13 (0.1 M KOH)) at a scan rate of 10 mV/s). 6.0 mg of each catalyst was dispersed in 1.49 mL of water, 0.57 mL of isopropanol, and 0.04 mL of a Nafion solution (5%). The catalyst ink was sonicated for one hour and 16.5 µL of catalyst ink drop-casted onto the desk electrode and then dried at room temperature. As a comparison, CV and LSV experiments in nitrogen saturated electrolytes were also performed. Electrochemical impedance spectroscopy (EIS)was carried out on a CHI760E working station. Stability test was obtained by a chronoamperometry measurement using RRED under 0.5V vs. RHE with a rotation speed of 1600 rpm for 10 hours. All potentials in this work were converted to reversible hydrogen (RHE) by the following equation (1),H2O2selectivity was calculated by equation (2)[34], and electronic transfer number was calculated by equation (3)[5].

where Idis the disk current, Irthe ring current, and N the collection efficiency (0.249).
3 RESULTS AND DISCUSSION
3. 1 Structure discussion
The Ta2O5/F-C catalyst was successfully synthesized by calcining PVDF and Ta2O5spheres in N2at 800 ℃. Figs. 1a and S1a show the SEM images with different magnification of the Ta2O5spheres which have a smooth surface and a particle size of tens to hundreds of nanometers. For comparison, the SEM image of Ta2O5-800 (Ta2O5spheres were calcined at 800 ℃) shown in Fig. S1b suggests that the morphology of Ta2O5sphere maintained after calcination.Figs. 1b and S1c suggest that the F doped C (F-C) displayed as a block shape. Compared with the Ta2O5sphere precursor,the rough surfaces of Ta2O5/F-C composite shown in Figs. 1c and S1d illustrate that the F doped C is coupled with Ta2O5sphere. The TEM image of Ta2O5spheres (Fig. 2a) further proves the Ta2O5spheres are dense of several smaller nanospheres, 30~100 nm in size. In Fig. 2b, the TEM structure of F doped C indicates that F-C has a porous layered structure. The TEM image of Ta2O5/F-C (Fig. 2c)further suggests that the Ta2O5sphere was coupled with a layer of F doped carbon. Fig. S2a~2c shows the results of five spots EDX data of Ta2O5/F-0.5C, Ta2O5/F-C and Ta2O5/F-2C, illustrating that the composite contains F, O, Ta,and C elements and the atomic ratios of C and Ta are 8:1,15:1, 31:1, respectively. This corresponds to the feed ratio of Ta2O5spheres and PVDF. Fig. S2d reveals the EDX data of Ta2O5-800 draw near to 2:5 which can further prove the presence of Ta2O5phase. The EDX result of F-C (Fig. S2e)shows that the atom ratio of F element is 1.5%.

Fig. 1. SEM images of (a) Ta2O5 spheres, (b) F doped carbon and (c) Ta2O5/F-C

Fig. 2. TEM images of (a) Ta2O5 spheres, (b) F doped carbon and (c) Ta2O5/F-C
The XRD (X-ray diffraction) patterns of Ta2O5(Fig. S3)before calcination show two wide diffraction peaks,suggesting that Ta2O5spheres synthesized at room temperature are amorphous phase[35]. The XRD pattern of F-C (in Fig. S3) shows a wide peak of graphite carbon. The X-ray diffraction (XRD) pattern of Ta2O5and Ta2O5/F-C (Fig. 3)mainly demonstrate the orthorhombic pattern of Ta2O5(ICSD No. 25-0922).

Fig. 3. XRD patterns of Ta2O5/F-C and Ta2O5-800
The high resolution XPS spectrum for C1s is shown in Fig. 4a, which reveals that the fitting peaks at 284.5, 286.2,288.2 and 289.8 eV are corresponding to C-C, C-O, C-F and O-C=O chemical bonds, respectively[36]. It confirmed that F atoms are incorporated into C matrix. The fitting peaks of O 1s spectrum (Fig. 4b) at 531.4, 530.1 and 533.1 eV are corresponding to C=O, O-Ta and O-C=O bonds, which demonstrates that O atoms are combined with C and Ta atoms[37,38]. The binding energy of the F 1s peak is 688.9 eV,which corresponds to F-C bond, as shown in Fig. 4c. This further indicates that fluorine is successfully doped into carbon after PVDF carbonization[36,37]. The Ta 4f7/2 and Ta 4f5/2 peaks in Fig. 4d are at 26.8 and 28.7 eV, which indicates the presence of Ta2O5[33].
The nitrogen adsorption-desorption isotherms of Ta2O5/F-C (Fig. 4e) demonstrate extremely rapid nitrogen absorption at very low relative pressures, indicating the typical microporosity property of Ta2O5/F-C[39]. In Fig. 4f,the BJH desorption pore-size distribution suggests that the pore width distribution is 1.16 nm. The BET surface area of Ta2O5/F-C is 152.6 m2/g and the micropore area is 140 m2/g with a micropore volume of 0.075 cm3/g. However,Ta2O5-800 has no conspicuous hysteresis loop at high relative pressure compared to Ta2O5/F-C, as shown in Fig. S4. Its BET surface area is only 8 m2/g and the pore volume is insignificant. As a result, it can be deduced that the increased BET surface area and pore volume of Ta2O5/F-C mainly comes from piled pore and porous F-C. The increased BET surface area not only exposes more catalytically active sites,but also improves mass transfer. This is more conducive to the production of hydrogen peroxide[40].

Fig. 4. X-ray photoelectron spectra of (a) C 1s, (b) O 1s, (c) F 1s and (d) Ta 4f for Ta2O5/F-C, (e) Nitrogen adsorption-desorption isotherms for Ta2O5/F-C and (f) BJH desorption pore-size distribution of Ta2O5/F-C
3. 2 Electrochemical discussion
The electrochemical performance measurement of the catalysts was based on rotating ring-disk electrode (RRDE)with a rotating speed of 1600 rpm in a three-electrode system.To better evaluate the ORR activity, the ring electrode is made of Pt to oxidize H2O2under a ring potential[41]. Fig. 5a and 5b reveals the cyclic voltammetry (CV) curves and the linear sweep voltammetry (LSV) profiles of the Ta2O5/F-C composites in N2and O2saturated alkaline electrolytes (0.1 M KOH solution). A remarkable increase of both the ring and disk currents in the presence of O2respect to the N2background was observed. The CV curve shows a flat slope in the N2saturated solution and an obvious reduction peak under O2saturated electrolyte, which indicates the reliability of oxygen reduction performance of Ta2O5/F-C.

Fig. 5. (a) CV and (b) LSV curves of Ta2O5/F-C in N2 and O2 saturated 0.1 M KOH solution
Fig. 6a shows the LSV curves of Ta2O5/F-C, Ta2O5-800 and F-C in 0.1 M KOH electrolyte. Obviously, the ring current of Ta2O5/F-C is the largest among all the three catalysts. Although Ta2O5-800 has a favorable H2O2selectivity, the oxygen reduction reactivity of Ta2O5-800 is poor. As shown in Fig. 6a and 6b, H2O2selectivity of Ta2O5-800 can reach nearly 70% but the limiting current density is just less than 1 mA/cm2and the onset potential at 0.64 V vs. RHE (defined as the potential at which a current density of 0.1 mA/cm2is achieved). The poor activity of Ta2O5-800 is ascribed to the lower electronic conductivity of Ta2O5[25]. As shown in Fig. 6b, the F-C has a poor H2O2selectivity about 55%, which is far less than the Ta2O5/F-C(80.8%). The resistance measurement further confirms the enhanced conductivity of the Ta2O5/F-C electrode. The high frequency range of EIS (Fig. S5) illustrated charge transfer ability for Ta2O5/F-C and Ta2O5-800. EIS in high frequency region (100 kHz to 10 Hz) was fitted with an equivalent circuit diagram to get charge transfer resistance. Obviously,the charge transfer resistance of Ta2O5-800 is two orders of magnitude larger than Ta2O5/F-C, which indicates the introduction of F-C improved the conductivity of Ta2O5successfully.
The LSV profiles of Ta2O5/F-0.5C, Ta2O5/F-C, and Ta2O5/F-2C that contain different ratios of F are shown in Fig. S6a. The Ta2O5/F-C displayed the highest disk current and ring current among the three catalysts, demonstrating that Ta2O5/F-C shows an excellent activity for two-electron ORR that is better than Ta2O5/F-C-0.5 and Ta2O5/F-C-2. The Ta2O5/F-C exhibits a high selectivity of H2O2of 80.8% at 0.49 V vs. RHE, and the selectivity is close to 80% within a wide potential range of 0.25~0.55 V. This catalyst also displays an excellent oxygen reduction activity with the onset potential of 0.78 V vs. RHE, which shows almost no overpotential. These efficient activity of Ta2O5/F-C surpass those of most other carbon support metal oxides in alkaline media (Table S1). The different selectivity shown in Fig. S6b can illustrate the feed ratio of C and Ta also play a nonnegligible role in the activity of such composites and the feed ratio of 1:1 is optimal. In Fig. 6a, F-C shows the largest disk current and the most positive onset potential among all catalysts, but the ring current is lower than Ta2O5/F-C. This unusual performance can be explained that the F-C tends to take four-electron ORR pathway to generate H2O. The H2O2selectivity of Ta2O5/F-C is better than that of F-C and Ta2O5,which demonstrates that F-C and Ta2O5propose a synergistic catalytic effect. Both the ring and disk currents were also obtained by RRDE in a neutral condition (0.1 M PBS solution with PH = 8) for Ta2O5/F-C and F-C (Fig. S7a). In Fig. S7b, Ta2O5/F-C shows a considerable performance for H2O2production with the selectivity of 68.5%, compared with the selectivity of 43.6% for F-C. Figs. 6c and S8 are the Tafel slopes for all the catalysts in different electrolytes.Obviously, Ta2O5/F-C has the lowest Tafel slope in alkaline electrolytes, so it shows the best kinetic rate than other catalysts. To evaluate its stability, a constant potential hold stability test at 0.5 V vs. RHE was performed by rotating ring-disk electrode at 1600 rpm. Fig. 6d shows that the ring and disk current density is rather stable during 10 h electrolysis for Ta2O5/F-C. Fig. S9 shows the H2O2selectivity and electron transfer number (ETN) of the catalysts after 10 h electrolysis. The H2O2selectivity kept around 80% and ETN is around 2.3 after electrolysis for 10 h.

Fig. 6. (a) LSV curves of Ta2O5/F-C, Ta2O5-800 and F-C (scan rate of 10 mV/s with a rotation speed of 1600 rpm).(b) H2O2 selectivity of Ta2O5/F-C, Ta2O5-800 and F-C in O2 saturated 0.1 M KOH electrolyte.(c) Tafel slopes for corresponding catalysts in O2 saturated 0.1 M KOH electrolyte.(d) Stability test for Ta2O5/F-C. All plots were subtracted from the nitrogen background current and the pH of test condition is 13
4 CONCLUSION
In summary, a synergistic effect is proposed to enhance the performance of Ta2O5/F-C composite catalysts for efficient H2O2electrosynthesis. The electrical conductivity of Ta2O5was significantly increased by forming Ta2O5/F-C interface.The Ta2O5/F-C catalyst shows an excellent selectivity more than 80% and long-term stability for H2O2production. The greatly enhanced performance of Ta2O5/F-C compared to F-C (selectivity of 59%) Ta2O5-800 (current density of 0.85 mA/cm2) counterparts were ascribed to the synergistic effect between F-C and Ta2O5. This work could provide a new way to rational design of carbon-supported metal oxide catalysts for H2O2electrosynthesis.
杂志排行
结构化学的其它文章
- A New Manganese Coordination Polymer Based on Azobenzene Tetracarboxylate and Auxiliary Pyridine Ligand: Synthesis, Crystal Structure and Magnetic Property①
- Urothermal Syntheses of Chiral Zincic Benzotriazole-5-carboxylate Frameworks for Iodine Uptake①
- Synthesis, Structure and Fluorescence Property of New Cd-MOFs Based on a Tetraphenylethylene (TPE) Ligand①
- Luminescent Lanthanide-titanium-organic Compound Constructed by Tetra-nuclear Ln-Ti Building Units and Diphenylglycolic Acid①
- Synthesis, Structure and Photophysical Properties of a Dinuclear Copper(I) Complex Based on Phosphinopyridine and Diphosphine Mixed-ligands①
- A Novel Co(II)-organic Framework with Multiple Active Sites for Selective Gas Adsorption①