Crystal Structure of Scheelite-type LiTb(WO4)2 and Multi-color Emitting Properties Doped by Eu3+①
2020-09-05XUEYaLiZHAODanCUIXiaoQiHANXiaoYangLIUBaoZhongFANYanPing
XUE Ya-Li ZHAO Dan CUI Xiao-Qi HAN Xiao-Yang LIU Bao-Zhong FAN Yan-Ping
(College of Chemistry and Chemical Engineering, Henan Polytechnic University, Jiaozuo 454000, China)
ABSTRACT Single crystal of lithium terbium tungstate LiTb(WO4)2 has been grown by the flux method. The crystal structure was refined from single-crystal X-ray data. It crystallizes in tetragonal system, space group I41/a with a = 5.1749(9), c = 11.1953(19) Å, V = 299.81(12) Å3, Z = 2, Mr = 661.56, Dc = 7.328 g/cm3, F(000) = 560, μ(MoKα) = 49.94 mm-1, R(F2 > 2σ(F2)) = 0.026 and wR(F2) = 0.070. It features a typical scheelite-type structure composed of two-direction packing of isolated WO4 tetrahedra. Li and Tb atoms in the structure occupy the same crystallographic site. Moreover, a series of solid solution phosphors LiTb1-xEux(WO4)2 (x = 0.004~0.1) were synthesized by high temperature solid-state reactions. The phosphors could be effectively excited by a wavelength range from 379 to 487 nm, which matches well with the UV and near-UV LED chip. The emission color of the phosphor can be tuned from green, through yellow to red by simply adjusting the relative Eu3+ and Tb3+ concentration due to the Tb3+ to Eu3+ energy transfer.
Keywords: rare earth compounds, crystal structure, optical properties, phosphor, charge transfer; DOI: 10.14102/j.cnki.0254-5861.2011-2405
1 INTRODUCTION
In recent years, rare-earth (Ln3+) activated phosphors have been widely used in modern society to meet the increasing need for the creative applications in everyday devices, such as TV screens, computer monitors, electronic billboards, portable electronics, and white light emitting diodes (WLED)[1-5]. Typically, the method of commercial white LEDs produced by Nichia Corporation is to combine a blue InGaN chip with a yellow phosphor YAG:Ce3+, wherein blue light excites the phosphor[6,7]. To improve the luminous efficiency, a new way which combined a near-ultraviolet (UV) LED chip with red, green and blue phosphors has been suggested. Such a combination can yield high color reproducibility and rendering index. Therefore, green and red phosphors with high thermal and chemical stability which can be excited by near UV around 400 nm attracted much attention in the past few years because of the amazing phenomenon of multi-color and tunable emission, such as K8Nb7P7O39:Eu3+[8], Ba3Y(PO4)3:Ce3+/Tb3+[9]and so on[10-13].
It is well-known that the energy transfer process usually has many effects on altering the luminescence intensity, color and lifetime of a phosphor[14]. As two famous Ln3+ions, Tb3+and Eu3+show intense green and red emissions due to the 4f→ 4ftransitions, respectively[9,15]. Moreover, Tb3+and Eu3+co-doped phosphors usually show an effective energy transfer from Tb3+to Eu3+, which have been produced many references[16-20]. However, the common feature of most reports is that Eu3+and Tb3+ions are co-doped in a third-party host, whereas Eu3+-doped terbium based compounds have rarely been reported.
Rare-earth double tungstate with the general formula ALn(WO4)2(A = Li, Na, K, Rb, Cs; Ln = Y, La-Lu) has attracted much attention for their applications as luminescent host materials[21-23]. Most of these crystals feature a scheelite-type structure with tetragonalI41/asymmetry at room temperature[24]. For LiTb(WO4)2, the structure can be thought as the substitution of two Ca2+ions in CaWO4by a couple of Li+and Tb3+ions in a statistical manner. Although the crystal structure of LiTb(WO4)2is characterized by powder X-ray diffraction analysis in the literature[25], no single crystal data have been given until now.
In this work, we report the single crystal growth and structure determination of LiTb(WO4)2. Moreover, a series of LiTb1-xEux(WO4)2(x= 0, 0.004, 0.008, 0.01, 0.02, 0.05, 0.08, 0.1) solid solutions were prepared, which show multi-color light emitting performance due to the efficient Tb3+→Eu3+charge transfer.
2 EXPERIMENTAL
2. 1 Materials and methods
All raw materials of Li2CO3(≥99.5%), WO3(≥99.9%), Eu2O3(≥99.95%) and Tb4O7(≥99.95%) were purchased from Sinopharm Chemical Reagent Shanghai limited company and used without any further purification. The X-ray powder diffraction (XRD) analysis was performed by Rigaku DMax2500 diffractometer with graphite- monochromatic CuKαcharacteristic radiation (2θ=5~70°). Photoluminescence spectra were carried out by FLS920 Edinburgh Analytical Instrument apparatus. The infrared absorption spectrum was recorded on a Perkin Elmer (FTIR 2000) spec- trometer in the change of 1000~450 cm-1. Sample in powder form was pressed into a disk using pellet of KBr.
2. 2 Synthetic procedure
Single crystals of LiTb(WO4)2were prepared by the high-temperature flux method by using Li2O-WO3as a flux. It was grown from a mixture of Li2CO3(0.3400 g, 4.6009 mmol), Tb4O7(0.4300 g, 0.5751 mmol), and WO3(2.0000 g, 8.6267 mmol) with the molar ratio of 8:1:15 in a 20 mL Pt crucible. The mixture was placed in a vertical programmable temperature furnace, and then heated at 900 ℃ and kept this temperature until the solution became transparent and clear enough in the open air, then cooled at a rate of 2 ℃·h-1to 600 ℃, to grow single crystals. Finally, the production was washed by hot water to dissolve the addition flux and then a few colorless crystals of high optical quality were obtained.
Powder sample of LiTb(WO4)2was prepared by the high-temperature solid state reaction method according to the following solid-state reactions:

The raw materials of Li2CO3(0.0797 g, 1.0785 mmol), WO3(1.0000g, 4.3134 mmol) and Tb4O7(0.4031g, 0.5391 mmol), with the stoichiometric molar ratio of 2:8:1, were thoroughly grounded and pressed into a pellet. Then the mixture was transferred into a proper platinum crucible and preheated at 500 ℃ for 5 h at a muffle furnace. After that, the mixture was ground again to guarantee the best homogeneity and then continue to heat to 800 ℃ for 48 h in the open air. In this stage, it is very important to grind and mix the mixture every ten hours to improve crystallinity. Moreover, powder samples of LiTb1-xEux(WO4)2(x= 0.004, 0.008, 0.01, 0.02, 0.05, 0.08, 0.1) were prepared by the same way according to the following solid-state reactions.


The purity of the powders was confirmed by powder XRD (2θ= 5~70°) analysis, as shown in Fig. 1. The experimental patterns were well indexed to the pure tetragonal phase of LiTb(WO4)2and no other phase was observed, which indicated that the powder samples are pure and the structure model is right.

Fig. 1. XRD patterns of solid solution LiTb1-xEux(WO4)2 (x = 0, 0.004, 0.008, 0.01, 0.02, 0.05, 0.08, 0.1) and simulated patterns of LiTb(WO4)2
2. 3 Crystallography
Several proper crystals (0.20mm × 0.05mm × 0.05mm) were selected and carefully mounted in fiberglass for single-crystal X-ray diffraction (SC-XRD) analysis. The set of intensity data was carried out using a Bruker Smart Apex2 CCD with graphite-monochromatic MoKα(λ= 0.71073 Å) radiation at 296 K. All of the atoms were refined with anisotropic thermal parameters. The important bond distances and bond angles are given in Table 1.

Table 1. Selected Bond Lengths (Å) and Bond Angles (°)
3 RESULTS AND DISCUSSION
3. 1 Crystal structure
SC-XRD analysis indicates that compound LiTb(WO4)2belongs to the tetragonal centrosym- metric space groupI41/aand exhibits a three- dimensional (3D) network consisting of two-direc- tion packing of isolated WO4tetrahedra and Li/Tb atoms (Fig. 2). The reason that Li and Tb atoms were expressed as Li/Tb is that they are disordered and randomly occupy the same 4a site. The Li|Tb atom is coordinated by eight oxygen atoms with Li/Tb-O bond distances ranging from 2.405(5) to 2.416(5) Å (Table 1). W atom locates at the center of a tetrahedron with the four equal W-O bond distances of 1.784(5) Å, and O-W-O bond angles fall in the range of 107.04(16)~114.5(3)°. These values are common compared with other reports[26-28].

Fig. 2. View of the crystal structure of LiTb(WO4)2 composed of [WO4] tetrahedra and (Li/Tb)2+ ions
3. 2 IR spectroscopic characterization
The Fourier transform infrared (FT-IR) spectrum of LiTb(WO4)2was recorded to characterize the structural detail, as shown in Fig. 3. A series of absorption peaks from 450 to 1000 cm-1originate from the vibrations of WO4tetrahedra. Among them, the bands at 874 and 515 cm-1can be assigned to stretching modes of W-O in WO4tetragon. The bands at 829 and 706 cm-1correspond to theν1andν3modes of the WO4tetrahedra, respectively. The band at 609.5 cm-1was due to the symmetrical vibrations of bridge oxygen atoms of Li/Tb-O-W groups[29,30]. The IR spectrum confirms the existence of tetrahedrally coordinated tungsten atoms, which is consistent with the results obtained from the single-crystal X-ray structural analysis.

Fig. 3. FT-IR spectra of the LiTb(WO4)2 sample
3. 3 Excitation and emission spectra
Fig. 4a shows the excitation spectra of undoped LiTb(WO4)2phosphor by monitoring green emission 547 nm (5D0→7F2) in the range of 200~500 nm at room temperature. There exist a series of narrow bands in the range from 315 to 390 nm, which can be assigned to the spin-forbidden 4f→4ftransitions of Tb3+:7F6→5D0(319 nm),7F6→5G2(341 nm),7F6→5D2(353 nm),7F6→5G5(360 nm),7F6→5G6(370 nm),7F6→5D3(379 nm) and7F6→5D4(487 nm), as listed in Table 2. The peak at 379 nm is the strongest, which is a common character compared with other reported phosphors[31,32]. Under excitation of 379 nm, four typical emission peaks from blue to red region are generated, which can be assigned to the5D4→7FJ(J= 3, 4, 5, 6) transition of Tb3+, that is, 491 nm (5D4→7F6) in the blue region, 547 nm (5D4→7F5) in the green region, and 589 nm (5D4→7F4) and 616 nm (5D4→7F3) in the red region. The strongest one is located at 547 nm, which is the reason why compound LiTb(WO4)2exhibits strong green emission. This result is essentially in agree- ment with other Tb3+activated phosphors, such as K2Ln(PO4)(WO4):Tb3+[31]and Li3Sc(BO3)2:0.01Tb3+[32].

Fig. 4. Excitation and emission spectra of LiTb(WO4)2 (a) and LiTb0.99Eu0.01(WO4)2 (b) phosphors
3. 4 Energy transfer between Tb3+ and Eu3+
The excitation and emission spectra of LiTb0.99Eu0.01(WO4)2at different excitation and emission wavelengths are given in Fig. 4b. It is obvious that the green emission of LiTb(WO4)2changes greatly when doped with Eu3+. The excitation spectrum by monitoring at 547 nm (5D4→7F5) is similar to undoped sample LiTb(WO4)2(Fig. 4a). By monitoring at 616 nm (5D0→7F2), the characterize excitation peaks of both Tb3+(319, 341, 353, 360, 370, 379, 487 nm) and Eu3+(395, 417, 465 nm) appear together (Table 2), indicating that an energy transfer occurs from Tb3+to Eu3+. On the other hand, the characterize emission peaks of both Tb3+(491, 547 nm) and Eu3+(594, 616, 656, 703 nm) appear together in the emission spectrum excited by monitoring at wavelength 379 nm (7F6→5D3), whereas by 395 nm (7D0→5L6) is similar to pure Eu3+samples or Eu3+doped materials[33-35]. This clearly proves that energy transfer takes place from Tb3+to Eu3+but the back transfer Eu3+→Tb3+does not exist in the LiTb0.99Eu0.01(WO4)2sample. It is a good property for solid solution phosphor LiTb0.98Eu0.02(WO4)2that a broad near-UV (350 ~400 nm) light can be strongly absorbed, which is nicely in agreement with the excitation wavelength around 400 nm for near-UV LEDs and blue LEDs in commercial LED, respectively[36-40].

Table 2. Excitation Peaks of LiTb1-xEux(WO4)2 Phosphors
To further investigate the energy, transfer process of Tb3+→Eu3+, the concentration-dependent lumine- scent properties of a serials of LiTb1-xEux(WO4)2(x= 0, 0.004, 0.008, 0.01, 0.02, 0.05, 0.08, 0.1) phosphors were studied. As shown in Fig. 5, all spectra reveal the characteristics of emission bands of Tb3+and Eu3+. Simultaneously, the emission spectrum clearly shows the decrease of Tb3+characterizes peaks (487, 547 nm) with increasing the Eu3+concentration from 0 to 0.1. On the contrary, the Eu3+characteristic emissions (595, 616, 656 and 703 nm) firstly increase with the increase of Eu3+concentration from 0 to 0.01, and then decrease when the concentration exceeds 0.01. There are two possible reasons for this phenomenon. One is the concentration quenching of excess Eu3+, and the other is that 378 nm is not more suitable than 395 nm[41,42].

Fig. 5. Emission spectra of representative LiTb1-xEux(WO4)2 (x = 0~0.1) phosphors excited by 379 nm (7F6 →5D3 of Tb3+) as a function of Eu3+ doping content x. Inset is the variatation of 547 nm (5D4→7F5 of Tb3+) and 616 nm (7F0→5D2 of Eu3+) emission intensity
It should be mentioned that the emission spectrum with 487 nm excitation (7F6→5D4of Tb3+) is similar with 379 nm (7F6→5D3of Tb3+) excitation spectra, enhancing the probability of Tb3+→ Eu3+energy transfer along with the increase of Eu3+dopant. The energy transfer efficiencies of LiTb1-xEux(WO4)2(x= 0.004, 0.008, 0.01, 0.02, 0.05, 0.08, 0.1) phosphors can be calculated by using the equation as follows[15,36]:

whereIandI0represent the 547 nm emission intensity of Tb3+host in the presence and absence of activator Eu3+[43]. The efficiency values were calculated to be 42.4%, 49.7%, 59.9%, 78.8%, 91.5%, 97.9% and 98.1% for Eu3+concentrations of 0.4%, 0.8%, 1%, 2%, 5%, 8% and 10%, respectively. We can see that the value is 59.9% with Eu3+concentration of 1%, and it increases significantly with increasing the Eu3+concentration until 5%, 59.9%→91.5%[31]. Then theηCT(I) values increase slowly, 91.5%→98.1%, for the Eu3+concentration of 5%→10%, showing the saturation of Tb3+→Eu3+charge transfer. This result suggests an efficient Tb3+→Eu3+charge transfer process and Eu3+is an excellent activator in LiTb(WO4)2host.
As shown in Fig. 6, the PL decay curve of LiTb1-x(WO4)2:xEu3+phosphors (excitation: 379 nm, emission: 547 nm) are well fitted with the single-exponential function[43,44]:

whereI0is the baseline correction,A1is a pre- exponential factor obtained from the curve fitting, andτis the lifetime of exciting state. The fittingτvalue is 2.46, 0.97, 0.91, 0.86, 0.61, 0.38, 0.22 and 0.14 ms for LiTb1-x(WO4)2:xEu3+samples withx= 0%, 0.4%, 0.8%, 1%, 2%, 5%, 8% and 10%, respectively. The luminescent decay lifetime of Tb3+emission at 547 nm decreased rapidly with increasing the concentration of Eu3+ions, indicating the existence of ET from Tb3+to Eu3+.

Fig. 6. Fluorescence decay profile for LiTb1-xEux(WO4)2 under the excitation of 379 nm
The energy transfer process between Tb3+and Eu3+ions is shown in Fig. 7. The electrons of Tb3+ions are excited by the 379 nm photons to their5D3level. Some of them relax to the7F6,7F5,7F4and7F3levels for generating the blue, green and red emissions, while the energy transfer is possible due to the nearby electrons of the Eu3+to the excited5D1,0level[45]. Subsequently, the electrons of Eu3+relax to the7FJ(J= 1~6) levels quickly, which generates the orange and red emissions. Notably, the characteristic emission of Eu3+is enhanced because of the effective overlap between5D4→7FJ(J= 3~6) emissions of Tb3+and the7F1→5D1,2absorption of Eu3+.

Fig. 7. Schematic diagram of the energy transfer between Tb3+ and Eu3+ in a host
3. 5 CIE chromaticity coordinates
Because the red emissions of Eu3+and green emissions of Tb3+simultaneously exist in solid solution materials LiTb1-xEux(WO4)2(x= 0~0.1) under UV or near-UV light excitation, the multi- color tunable luminescence can be obtained by adjusting thexvalue. The color of any light can be represented as an (x,y) coordinate on the basis of Commission International de L'Eclairage (CIE) functions. As shown in Fig. 8, the luminescent color (excited by 379 nm) tuned from green, yellow, orange to red as the concentration of Eu3+increases from 0 to 10% and the corresponding CIE coor- dinates are listed in Table 3. The other noteworthy thing is that the CIE chromaticity coordinate of LiTb0.9Eu0.1(WO4)2is so close to the standard red chromaticity coordinates (0.667, 0.330) of the National Television System Committee (NTSC). These presented results indicate the potential appli- cation of LiTb1-xEux(WO4)2phosphors for white- LEDs.
4 CONCLUSION
In summary, a single crystal of LiTb(WO4)2was prepared using high-temperature molten salt method and structurally determined through single-crystal X-ray diffraction analysis. The results show that it features the scheelite-type structure and crystalizes in the tetragonal space groupI41/a. Li+and Tb3+ions in the structure are disordered and randomly occupy the same site with the molar ratio of 1:1. A series of LiTb1-xEux(WO4)2phosphors were prepared via a high-temperature solid-state reaction method. Due to the concentration-dependent energy transfer, the emission color of the phosphor can be continuously changed from green through yellow and eventually to red by changing the doping concentration of Eu3+because of the energy transfer from Tb3+to Eu3+ions. Hence, we think that the as-prepared multicolor tunable phosphors could be a promising candidate for near UV convertible phosphor for LED and display applications.

Table 3. CIE Chromaticity Coordinates of LiTb1-xEux(WO4)2

Fig. 8. CIE chromaticity diagram for the emission spectra of LiTb1-xEux(WO4)2 samples excited by 379 nm and inset digital photograph of the emission from samples
杂志排行
结构化学的其它文章
- Theoretical Insights into the Substituent Effects on the Fluorescence of Boron Complexes of 2-(Benzothiazol-2-yl)phenols: a Quantum Mechanics Study①
- Interface Reconstruction Study by Functional Scanning Probe Microscope in Li-ion Battery Research①
- Syntheses, Crystal Structures and DNA-binding Properties of Cd(II), Co(II), Cu(II) and Zn(II) Complexes Containing Imidazolium Derivatives
- Hydrothermal Synthesis, Crystal Structure and Luminescence Property of a New Binuclear Cage-like Samarium(III) Complex Sm2(C7H4ClCOO)6(C12H8N2)2(H2O)2①
- A Chinese Lantern-like 2D Cu(II) Coordination Polymer Constructed by Bis-imidazole and Dicarboxylate Co-ligands: Synthesis, Crystal Structure and Photocatalytic Activity①
- Hydrothermal Syntheses, Crystal Structures and Luminescence Properties of Zn(II) and Cu(II) Complexes Based on 2,2΄-((Sulfonylbis(4,1-phenylene))bis(oxy))diacetic Acid①