原子层沉积二硫化钼薄膜的机理及生长薄膜的质量
2017-10-12黄亚洲沙菁陈云飞
黄亚洲 刘 磊 沙菁 陈云飞
(东南大学机械工程学院, 南京210096)
原子层沉积二硫化钼薄膜的机理及生长薄膜的质量
(东南大学机械工程学院, 南京210096)
选择MoCl5和H2S作为前躯体,Si和Al2O3作为基底,利用原子层沉积制备高质量的MoS2薄膜. 利用X射线能谱仪,对在温度450~490 ℃下所生长的薄膜进行分析,分析结果表明,氧化铝更适合薄膜的生长,460 ℃是最佳的生长温度. 利用扫描电子显微镜、X射线衍射仪、拉曼光谱和透射电子显微镜对所生长薄膜的形态和晶体结构进行研究.结果表明,所生长的薄膜厚度均匀一致,100个循环后,薄膜厚度约为20 nm,薄膜的平均生长率为0.2 nm,表面成花瓣片状结构. 所生长的2H-MoS2薄膜,其(002)晶面平行于基底,(002)、(100)、(110)晶面的间距分别为0.62,0.28和0.17 nm,具有完美的六方晶体结构.
MoS2薄膜;原子层沉积;生长温度;晶体结构
Abstract: MoS2films were prepared by atomic layer deposition using MoCl5and H2S as precursors, while Si and Al2O3were used as substrates, respectively. The thin films grown at different temperatures from 450 to 490 ℃ were observed by EDS (energy dispersive spectrometer). The results show that 460 ℃ is the most suitable growth temperature and the Al2O3substrate is more suitable than Si as a substrate. The morphologies and the crystal structures of the thin films were studied by SEM (scanning electron microscope), XRD (X-ray diffraction), Raman spectroscopy, and TEM (transmission electron microscope). The results show that the surface of the uniform film is a petal like structure and the film thickness by 100 cycles is about 20 nm. The grown MoS2is 2H structure and the (002) crystal plane is parallel to the substrate. It is clear thatd002,d100andd110for lattice planes (002), (100) and (110) are 0.62, 0.28 and 0.17 nm, respectively. Furthermore, the average growth rate of the high crystallinity MoS2film is 0.2 nm.
Keywords: MoS2thin films; atomic layer deposition; growth temperature; crystal structure
近年来,MoS2由于其优异的性能而引起了广泛的关注. MoS2是一种二维层状过渡金属半导体材料,层与层之间通过范德华力堆叠在一起,层内S原子和Mo原子通过强的化学键连接.
与石墨烯不同,MoS2的带隙结构随着层数的变化而变化,当MoS2从体态结构变为单层结构时,由间接带隙变为直接带隙. 由于MoS2具有重要的机械、电气和光学性能,MoS2在电化学器件、光电器件、氢存储、催化、电容器、固体润滑剂等领域具有重大的应用价值[1-5].
通常情况下,MoS2薄膜可以通过机械剥离的方法获得,但该方法效率低,且不易得到大尺寸的薄膜,因而该方法不能满足现代大规模集成电路的需要[6-8].人工合成制备大面积……