焊接挤压辊造成管体表面缺欠的处理
2017-10-11介升旗吴鹏飞陈浩明
介升旗,吴鹏飞,陈浩明
(宝鸡石油钢管有限责任公司 宝鸡专用管公司,陕西 宝鸡721008)
焊接挤压辊造成管体表面缺欠的处理
介升旗,吴鹏飞,陈浩明
(宝鸡石油钢管有限责任公司 宝鸡专用管公司,陕西 宝鸡721008)
为了有效消除高频直缝焊管管坯外表面的压痕和划伤缺欠,结合高频焊管机组焊接挤压辊的设计特点,分析了焊接挤压辊造成管坯压痕或划伤等表面缺欠的原因,认为上挤压辊辊缘对管坯造成线状压痕或压坑、侧挤压辊辊缘对管坯造成线性压痕或月牙状划伤、下辊辊缘对管坯造成线性压痕是造成表面缺欠的主要原因。通过对焊接挤压辊造成管坯表面缺欠原因的分析,提出了相应的防止措施。
高频焊;焊接挤压辊;压痕;划伤
Abstract:In order to effectively eliminate the dents and scratch defects on outer surface of high frequency longitudinal welded pipe billet,combined with the design characteristic of high frequency welded pipe units welding squeezing roller,it analyzed the main reasons for dents and scratch defects caused by welding squeezing roller.The results indicated that linear indentation or dents on pipe billet caused by upper squeezing roller edge;linear dents or crescent scratch on pipe billet caused by lateral squeezing roller edge;linear dents on pipe billet caused by lower roller edge.Through comprehensive analysis on the reasons of pipe billet surface defects due to welding squeezing roller,the corresponding preventive measures were put forward.
Key words:HFW pipe;welding squeezing roller;indentation;scratch
宝鸡石油钢管有限责任公司宝鸡专用管公司高频焊管机组生产外径为Φ193.7 mm的高频焊接管坯用于生产热张力减径油套管,该机组焊接挤压辊采用五辊挤压,在设备调试过程中管坯经过焊接挤压辊时,在管坯外表面造成线状压痕或月牙形划伤等表面缺欠。为了有效消除管坯外表面的压痕和划伤缺欠,从轧辊的孔型设计特点、安装精度以及轧辊参数设定等方面对可能产生压痕和划伤的原因进行了分析,针对压痕和划伤产生的原因提出的了相应的防止措施,消除了管坯压痕和划伤的产生,提高了管坯的表面质量。
1 焊接挤压辊的设计特点
焊接挤压辊采用五辊挤压,上挤压辊的孔型半径106.80 mm,侧挤压辊和下挤压辊孔型半径为97.09 mm。……