稀土La2O3对重力条件下复合陶瓷钢管陶瓷内衬组织的影响
2016-01-12刘宇雁,徐国芳,陈林
稀土La2O3对重力条件下复合陶瓷钢管陶瓷内衬组织的影响*
刘宇雁徐国芳陈林
(内蒙古科技大学材料与冶金学院内蒙古 包头014010)
摘要根据铝热反应,研究了复合陶瓷钢管重力条件下制备含SiO2系列陶瓷内衬,以及含稀土La2O3加SiO2系列陶瓷内衬等添加物对金属陶瓷内衬显微硬度和耐蚀性的影响。研究结果表明:当加入稀土La2O3和SiO2时均可使陶瓷层内衬的孔隙率降低,当La2O3和SiO2的加入量分别为0.5%和2.0%时,对陶瓷层性能的提高效果最好,使孔隙率降低至3%,耐蚀性达到0.06g/m2·h,在一定程度上使陶瓷内衬的耐蚀性增加,La2O3对提高陶瓷层性能的效果较好。
关键词稀土陶瓷内衬硬度耐蚀性
作者简介:*刘宇雁(1963-),教授、硕士生导师;主要从事材料新工艺、新技术的研究。
中图分类号:TG335
The Effect of Rare-earth La2O3on the Ceramic-lined Tissue of Composite Ceramic Tube under the Condition of Gravity
Liu Yuyan, Xu Guofang, Chen Lin(School of Material and Metallurgy,Inner Mongolia University of Science & Technology,Inner Mongolia,Baotou,014010)
Abstract:In this article the preparation containing SiO2 series ceramic-lined has been studied under the condition of composite ceramic tube gravity. And the effect of additives on the microhardness and corrosion resistant of metal ceramic-lined has been researched. These additives are rare-earth La2O3 and SiO2 series ceramic-lined. The experiment result showed that adding rare-earth La2O3 and SiO2 can make the porosity of ceramic layer lining to reduce. When the quantity of La2O3 and SiO2 were 0.5% and 2.0% respectively, the effect on the improvement of the performance of the ceramic layer was best, it made the porosity fall to 3% and the corrosion resistance reach 0.06g/m2·h. To some extent the corrosion resistance has been increased. La2O3 had a good effect to improve the performance of the ceramic layer.
Key words:Rare earth; Ceramic-lined; Hardness; Corrosion resistance
前言
复合陶瓷钢管是指采用自蔓延高温合成方法,将钢管内壁涂覆一层陶瓷材料。这种陶瓷内衬钢管具有耐磨、耐蚀、耐高温性能,是一种理想的管道输送材料,被广泛应用于石油、冶金、化工、矿山等领域。随着陶瓷衬管的大量使用人们对其表面质量和力学性能的要求也越来越高。笔者主要研究了Fe2O3+Al体系重力条件下陶瓷衬管组织演变规律,以及稀土镧对复合陶瓷钢管陶瓷内衬组织的影响。
1实验原理及方法

2实验结果分析
2.1Fe2O3+Al+SiO2系列陶瓷衬组织结果及分析
表1为添加SiO2的陶瓷层性能。

表1 添加SiO 2的陶瓷层性能

图1 含量为5%SiO 2的陶瓷层显微组织图
从制备的陶瓷复合管上切割出样品,经磨平、抛光制成试样,用10mol 3%的硝酸酒精加入1g的苦味酸进行腐蚀,然后在蔡司CA25型金相显微镜下进行金相组织观察结果见图1;……