Infuence of solution treatment on microstructure,mechanical and corrosion properties of Mg-4Zn alloy
2015-02-16HongminJiaXiaohuiFengYuanshengYang
Hongmin Jia,Xiaohui Feng,Yuansheng Yang*
Institute of Metal Research,Chinese Academy of Sciences,Shenyang 110016,China
Infuence of solution treatment on microstructure,mechanical and corrosion properties of Mg-4Zn alloy
Hongmin Jia,Xiaohui Feng,Yuansheng Yang*
Institute of Metal Research,Chinese Academy of Sciences,Shenyang 110016,China
The solution treatment parameters,mechanical properties and corrosion behavior of binary Mg-4Zn alloy were investigated.The results showed that after the solution treatment at 335°C for 16 h,Mg-4Zn alloy had an ultimate tensile strength of 184.13 MPa and elongation of 9.43%. Furthermore,the corrosion resistance was evaluated by electrochemical measurements and immersion tests in 3.5%NaCl solution.The results revealed that the corrosion current density of the solution treatment Mg alloy was 11.2 μA/cm−2,it was lower than 15.8 μA/cm−2for the as-cast Mg alloy under the same conditions,which was greatly associated with the micro-cathode effect of the second phases.
Solution treatment;Magnesium alloy;Mechanical property;Corrosion behavior
1.Introduction
Magnesium alloys have attracted great attention as medical implant material and devices due to their low density,perfect biocompatibility and close mechanical properties to natural bone[1–3]and it is also naturally found in the human body, where it plays essential roles in metabolic pathway[4–7]. Various magnesium alloys have been researched as biodegradable materials,such as AZ31,AZ91,AE21,WE43,LAE442 and so on[8,9].Unfortunately,most of the reported biomedical magnesium alloys contain aluminum and/or rare earth elements.Many researches[10–13]have shown Al is harmful to neurons and osteoblasts and also associated with dementia and Alzheimer’s disease.The administration of RE could lead to hepatotoxicity[14].Song explored several Mg alloys,pointing out that Zn,Ca and Mn could be appropriate element for biomedical application[6].It was also found that zinc was one of the most abundant nutritionally essential elements in the human body and had basic safety for biomedical application[12]. Therefore,Zn-containing Mg alloys have been paid more attention and developed as promising biomaterials.
However,the application of Mg alloys has been limited due to their high corrosion rate at physiological conditions and their fast biodegradation before the new tissue has adequately been healed[15].The early researches[16–21]have indicated that the poor corrosion resistance of Mg alloys mainly results from two reasons:The frst is the intrinsic dissolution tendency of magnesium,which is only weakly inhibited by corrosion product flms;the second is the presence of second phases acting as local cathodes and thus causing local micro-galvanic to accelerate corrosion[15].The effect of second phases on the corrosion resistance of Mg alloys has been investigated widely [22–27],especially for theAZ91 Mg alloys.The second phases usually act as cathodes to accelerate corrosion,while they may act as barrier against corrosion if they are in the form of continuous network along grain boundaries.In general,heat treatment is the most effective method to adjust the second phases, corresponding to change in the properties of Mg alloys[23].In this paper,the most suitable parameter of solution treatment is discussed and the effects of solution treatment on mechanical and corrosion properties of Mg-4Zn alloy as a degradable biomaterial are investigated to clarify the role of second phases in the corrosion mechanism.
2.Experimental
Ingots with nominal alloy compositions of Mg-4wt%Zn alloy were prepared with pure magnesium(99.99 wt%)and pure zinc(99.99 wt%)in an electronic resistance furnace underthe protection of CO2and 0.8%SF6mixture gas.The alloying melt was held at 730°C for 30 minutes to homogenize,and cast as ingots at 690°C into a graphite mold.The chemical compositions of the alloy were measured by inductively coupled plasma atomic emission spectrum (ICP-AES) apparatus.
还好,我脑海中不断显现的尴尬局面并没有在第一天的傍晚出现,为第二天正式拍摄的探路工作在浅尝辄止之后就结束了。而为了让我在第二天不成为整个拍摄计划的最主要障碍,牧马人车主自告奋勇地开始帮我复习曾在各种“冰雪试驾”和“越野体验”活动中收获的知识点。一番理论教授结束之后,在一群改头换面的北汽BJ40、三菱帕杰罗的围观下,我成功依靠全新AMG G 63那充沛到有些过剩的动力摆脱了一个因为掉头而陷入雪窝的尴尬。
Specimens cut from the ingots were frst solution treated with different times,then quenched into water.The temperature of solid solution was determined by the Mg-Zn binary phase diagram[28]and DSC analysis.Microstructures of specimens for different heat treatment times were observed with an optical microscope(OM).Vickers hardness testing was taken using 100 g load and holding time of 10 s,not fewer than 5 points were taken in each specimen.Tensile tests were performed at room temperature and a constant cross-head speed of 1 mm s−1. Three specimens were used for same test conditions to ensure the reproducibility of data.
[1]Y.F.Zheng,X.N.Gu,F.Witte,Mater.Sci.Eng.R 77(2014)1–34.
Samples for electrochemical test were cut from the ingots and mounted by epoxy resins with an exposed area of 1 cm2. The surface was grinded by 600–2000#SiC papers.The polarization test was carried out at room temperature in a beaker containing 3.5%NaCl solution using a standard three electrode confguration:the saturated calomel as a reference,a platinum electrode as the counter and the sample as the working electrode.In the polarization tests,the working electrode was frst immersed in NaCl solution for 5 minutes and then the polarization curve was measured at a scanning rate of 0.5 mV/s.
This work has been concerned with the solution treatment parameters,mechanical and corrosion properties.The main results can be summarized as follows.
3.Results and discussion
3.1.The optimum solution treatment parameters
The optical microstructure and XRD results of the as-cast Mg-4Zn alloy are shown in Fig.1.It can be seen that there were two main phases in the as-cast samples,namely,the matrix α phase and the second phases MgZn,precipitating along the grain boundary.
The DSC curves of the Mg-4Zn alloy are shown in Fig.2,the second phases dissolve at 346°C and exist steadily below 329°C.So the solid solution treatment temperature wasdetermined at 335°C in consideration of the furnace temperature fuctuation.
(一)在主推品种方面 武隆县在肉牛产业发展中,主推西门塔尔牛和安格斯牛,首先用西门塔尔牛冷冻精液配种川南山地黄牛经产母牛,再用安格斯牛冻精配种“西杂牛”,并将“红西本”三杂牛作为商品牛进行育肥出售。

Fig.1.Microstructure of the as-cast Mg-4Zn alloy and XRD result.

Fig.2.The DSC curve of Mg-4Zn alloy.
The curve of micro-hardness variation of the Mg-4Zn alloy for solution treatment at 335°C with time is shown in Fig.3. The hardness values are increased as solution time and reached a peak at 16 h,then the hardness started to decrease gradually. The change of the hardness can be explained through the microstructures during the solution treatment which are shown in Fig.4.It can be seen from Fig.4a and b that the microstructures contain a large number of second phases and the second phases become more dissolved into the Mg matrix with the increasing solution time(Fig.4c).By a solution time of 16 h,the second phases are dissolved completely(Fig.4d)and the alloy has a supersaturated single phase.There is a noticeable coarsening tendency of the grains in the following time(Fig.4e and f) compared with that of the original microstructure.As a result, the optimum solution parameter should be 335°C for 16 h for the Mg-4Zn alloy in the experiments.

Fig.3.Variation of the micro-hardness with solution time.
3.2.The effect of solution treatment on the mechanical properties
古往今来,传统文化一直是我们日常生活中的一部分,它贯穿了我们每个人的人生阶段,它是无形的,亦是有形的。但如何理解这份传统文化呢?
The tensile properties of the as-cast Mg-4Zn alloy in comparison with solution treatment Mg alloy are summarized in Table 1.The ultimate tensile strength(UTS)and elongation of the as-cast Mg alloy are 156.93 MPa and 7.38%,respectively. However,after the solution treatment,the UTS and elongation increased to 184.13 MPa and 9.43%,respectively.The enhancement of UTS is due to the solution strength effects of the alloying elements.Besides,Zn dissolving into Mg matrix will decrease the stacking fault energy of the matrix,which leads to the change of plastic deformation mechanism,i.e.,cross slip is diffcult to happen and twins will appear to adjust plastic deformation[29].Thus,the solution treatment will enhance the UTS and elongation at the same time.
The SEM micrographs of the fracture surface of the Mg-4Zn alloy are illustrated in Fig.5.The fracture surface consists of cleavage planes for the as-cast Mg-4Zn alloy(Fig.5a),which is in accordance with its lower elongation of 7.38%,so the fracture mold of as-cast Mg-4Zn alloy is quasi-cleavage.For the alloy subjected to solution treatment at 335°C,the fracture surface contains dimples and tear ridges(Fig.5b),which is in accordance with its higher elongation of 9.43%.But the fracture mold is also quasi-cleavage.
目前我国人民银行、存款保险基金管理机构、银监部门都可以依法对问题银行采取早期纠正和风险处置措施,省级地方政府对农信社负有管理责任和风险处置责任。可建立存款保险管理机构、人民银行、银行业监管管理机构、省级地方政府等共同参与的问题银行市场退出磋商机制,加强监管协调和信息共享,强化协同推进,提高问题银行风险处置的效率。此外,还应进一步明确存款保险管理机构运用存款保险基金参与问题银行接管、重整、破产等风险处置的形式和职责范围,加强相关法律法规之间的有效衔接,完善问题银行市场化退出机制。……
杂志排行
Journal of Magnesium and Alloys的其它文章
- GUIDE FOR AUTHORS
- Infuence of sulfate ion concentration and pH on the corrosion of Mg-Al-Zn-Mn(GA9)magnesium alloy
- Research of growth mechanism of ceramic coatings fabricated by micro-arc oxidation on magnesium alloys at high current mode
- Effect of experimental parameters on the micro hardness of plasma sprayed alumina coatings on AZ31B magnesium alloy
- Electrochemical deposition of Mg(OH)2/GO composite flms for corrosion protection of magnesium alloys
- Effect of temperature and strain rate on compressive response of extruded magnesium nano-composite